Activated lithium salt solid waste for ultra-high performance concrete as well as preparation method and application of activated lithium salt solid waste
By using activated lithium salt solid waste and composite activators in ultra-high performance concrete, the surface structure and internal voids of lithium salt solid waste powder are improved, and the problems of easy agglomeration of lithium salt solid waste and slow early hydration reaction are solved, and the problem of high-performance concrete is improved. The strength and stability of concrete achieve efficient utilization of lithium salt solid waste.
Patent Information
- Application Number
- CN202411029837.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
During the molding process, ultra-high performance concrete has a large slurry viscosity and difficult to eliminate bubbles, resulting in volume instability and durability problems. The surface of lithium salt solid waste powder is porous and prone to agglomeration, and the early hydration reaction is slow, affecting performance.
Use activated lithium salt solid waste, mix and grind it with lithium salt solid waste powder by mixing and grinding it with composite activators composed of triethanolamine, sodium sulfate, sodium silicate, calcium formate, calcium nitrate, chitosan, etc. to improve its surface structure and internal space. , promote early strength improvement of cement and bubble discharge.
Effectively neutralize trace acidic substances in lithium salt solid waste, optimize the combination of lithium salt solid waste and cement, improve the strength and stability of ultra-high performance concrete, reduce production costs, and realize the resource utilization of green and low-carbon solid waste.
Smart Images

Figure CN118993607A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of building cementitious materials, and in particular to activated lithium salt solid waste for ultra-high performance concrete, and a preparation method and application thereof. Background Art
[0002] As the metal with the lowest density, lithium has unique physical and chemical properties. Lithium resources are widely used in the fields of lithium battery production, alloy production, optical materials, etc. The currently widely used method for extracting lithium from spodumene is sulfuric acid roasting. This method has a high content of lithium in spodumene and requires spodumene to be first subjected to a beneficiation process. The overall production cost is high, and the waste residue produced contains calcium sulfate, which can cause problems such as poor durability of concrete when added to concrete. Chinese patents CN115321563A, CN114854986A, and CN115286019A disclose a method for extracting lithium resources by nitric acid pressure leaching of spodumene. The obtained lithium salt solid waste powder has obvious volcanic ash activity and only a trace amount of acid residue, which can be used to prepare concrete admixtures and replace silica fume and fly ash in some ultra-high performance concrete formulas.
[0003] Ultra-high performance concrete has been applied in many fields such as bridges, super high-rise buildings, and component repairs due to its high strength, high toughness, and high durability, and has good development prospects. However, due to the low water-binder ratio of ultra-high performance concrete, the slurry has high viscosity during the molding process, and it is difficult to eliminate the bubbles in the slurry, which has an adverse effect on the volume stability and durability of ultra-high performance concrete.
[0004] Due to the particularity of the front-end process of nitric acid pressure leaching of lithium salt solid waste, the lithium salt solid waste powder itself has the characteristics of porous surface. After adding cement, it is easy to agglomerate and the early hydration reaction is slow. The gas remains in the lithium salt solid waste powder, which is more difficult to discharge during the ultra-high performance concrete molding process. In addition, trace acidic substances are likely to remain in the micropores of lithium salt solid waste, which will lead to the deterioration of concrete performance in the later stage. At the same time, due to its front-end nitric acid pressure leaching process, compared with the sulfuric acid method leaching lithium slag, only trace amounts of Ca 2+ When mixed with cement, it causes the cement hydration capacity to decrease, thus affecting the performance of ultra-high performance concrete. Summary of the invention
[0005] Based on the above problems, the present invention provides activated lithium salt solid waste for ultra-high performance concrete, and a preparation method and application thereof, which can promote the improvement of cement early strength and other properties, and can achieve the improvement of the surface structure of lithium salt solid waste powder, solve the problem of easy agglomeration of lithium salt solid waste, and optimize the combination of lithium salt solid waste powder and cement, improve the problem of the difficulty of filling lithium salt solid waste inside, resulting in the presence of bubbles inside the ultra-high performance concrete matrix and difficulty in discharging bubbles, which helps to improve the strength performance and stability of lithium salt solid waste-based ultra-high performance concrete (UHPC).
[0006] In order to achieve the above technical effects, the technical solution adopted by the present invention is:
[0007] An activated lithium salt solid waste for ultra-high performance concrete, comprising lithium salt solid waste powder and a composite activator, wherein the lithium salt solid waste powder is a solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid;
[0008] The composite activator comprises a composite formed by component A and component B, wherein:
[0009] Component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid;
[0010] Component B comprises a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
[0011] Furthermore, the chemical components of the lithium salt solid waste include: 70-75% SiO2, 20-25% Al2O3, 0.05-0.4% CaO, 0.01%-5% impurity oxides, and the impurity oxides are a combination of one or more oxides of Fe2O3, K2O, and MgO.
[0012] Furthermore, the mass ratio of each raw material in component A is 30:24:45:1 of triethanolamine:sodium sulfate:sodium silicate:grinding aid, and the mass ratio of each raw material in component B is 19:25:55:1 of calcium formate:calcium nitrate:chitosan:grinding aid.
[0013] Furthermore, the average particle size of the activated lithium salt solid waste ranges from 1.48 μm to 3.28 μm.
[0014] In order to achieve the above technical effects, the present invention also provides a method for preparing activated lithium salt solid waste for ultra-high performance concrete, comprising:
[0015] The solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid is dried to obtain lithium salt solid waste powder;
[0016] The lithium salt solid waste powder and the composite activator are mixed and ground, and aged for at least 3 hours after the grinding is completed to obtain the activated lithium salt solid waste; the composite activator includes a complex formed by component A and component B, wherein: component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid; component B includes a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
[0017] Furthermore, the chemical components of the lithium salt solid waste include: 70-75% SiO2, 20-25% Al2O3, 0.05-0.4% CaO, 0.01%-5% impurity oxides, and the impurity oxides are a combination of one or more oxides of Fe2O3, K2O, and MgO.
[0018] Furthermore, the mass ratio of each raw material in component A is 30:24:45:1 of triethanolamine:sodium sulfate:sodium silicate:grinding aid, and the mass ratio of each raw material in component B is 19:25:55:1 of calcium formate:calcium nitrate:chitosan:grinding aid.
[0019] Furthermore, the lithium salt solid waste powder and the composite activator are mixed and ground to an average particle size range of 1.48 μm to 3.28 μm, and the activated lithium salt solid waste is obtained after aging for at least 3 hours.
[0020] In order to achieve the above technical effects, the present invention also provides a method for preparing ultra-high performance concrete using activated lithium salt solid waste, comprising:
[0021] In parts by weight, 625 to 700 parts of cement, 65 to 110 parts of fly ash, 70 to 140 parts of silica fume, 70 to 180 parts of activated lithium salt solid waste, 900 to 1000 parts of quartz sand, 155 to 175 parts of water, and 10 to 17 parts of a water reducing agent are stirred and mixed to obtain a mixed material; the activated lithium salt solid waste is the activated lithium salt solid waste for ultra-high performance concrete;
[0022] 50-100 weight of steel fibers are added to the mixture and stirred evenly before pouring and forming. After curing to a specified age, ultra-high performance concrete using activated lithium salt solid waste is obtained.
[0023] Furthermore, the steel fiber is a copper-plated straight wire steel fiber with a length of 12 to 14 mm and a diameter of 0.18 to 0.23 mm; during the curing process to the specified age, the curing system is: after casting and forming, it is cured for 1 day under the conditions of a temperature of 20°C and a humidity of more than 90%, and then demolded, and placed in an environment with a temperature of 20±2°C and a humidity greater than 95% for standard curing to the specified age.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The triethanolamine and chitosan in the activated lithium salt solid waste of the present invention can effectively neutralize the trace acidic substances remaining in the lithium salt solid waste to prevent the expansion and deterioration of concrete; calcium formate and calcium nitrate can provide Ca 2+ , in order to ensure the ultra-high performance concrete mixture environment Ca 2+The concentration is normal, which promotes the improvement of cement's early strength and other properties. On this basis, calcium ions complex with polar groups in chitosan to form coordinated covalent bonds, which can not only improve the mechanical properties of chitosan, but also further promote the dissolution of calcium ions, making the calcium ion concentration in the early liquid phase reaction significantly increased. In addition, the radius of chitosan particles is larger than that of calcium ions, making it easier to generate smaller complexes with a coordination number of 6. Under the induction of the template effect, CO3 2- Rapidly with Ca 2+ Combined with the formation of calcite-type calcium carbonate (coordination number 6), thereby inducing the massive formation of calcite. In addition, the addition of chitosan itself will also improve the anti-deterioration ability of ultra-high performance concrete materials.
[0026] 2. The activated lithium salt solid waste of the present invention uses composite activator particles to adhere to the surface of lithium salt solid waste or enter its internal voids, and closely combine with lithium salt solid waste particles, thereby improving the surface structure of lithium salt solid waste powder, solving the problem of easy agglomeration of lithium salt solid waste, and optimizing the combination of lithium salt solid waste powder and cement. In the cement hydration process, hydration products such as calcite will preferentially grow on the surface or voids with composite activator particles, which is not only conducive to the discharge of air inside the voids of lithium salt solid waste, but also improves the problem that bubbles exist inside the ultra-high performance concrete matrix due to the difficulty of filling lithium salt solid waste and are difficult to discharge, and further strengthens the combination between lithium salt solid waste and hydration products, which helps to improve the strength performance and stability of lithium salt solid waste-based ultra-high performance concrete (UHPC). BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a SEM image of activated lithium salt solid waste powder with an average particle size of 1.48 μm;
[0028] Figure 2 is the SEM image of untreated lithium salt solid waste powder;
[0029] Figure 3 This is a SEM image of UHPC doped with activated lithium salt solid waste powder with an average particle size of 1.48 μm. DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0031] Example 1
[0032] An activated lithium salt solid waste for ultra-high performance concrete, comprising lithium salt solid waste powder and a composite activator, wherein the lithium salt solid waste powder is a solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid;
[0033] The composite activator comprises a composite formed by component A and component B, wherein:
[0034] Component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid;
[0035] Component B comprises a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
[0036] In this embodiment, the method for preparing activated lithium salt solid waste for ultra-high performance concrete includes:
[0037] The solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid is dried to obtain lithium salt solid waste powder;
[0038] The lithium salt solid waste powder and the composite activator are mixed and ground, and aged for at least 3 hours after the grinding is completed to obtain the activated lithium salt solid waste; the composite activator includes a complex formed by component A and component B, wherein: component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid; component B includes a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
[0039] In this embodiment, the triethanolamine and chitosan in the activated lithium salt solid waste can effectively neutralize the trace acidic substances remaining in the lithium salt solid waste to prevent the expansion and deterioration of concrete; the calcium formate and calcium nitrate in component B can provide Ca 2+ , in order to ensure the ultra-high performance concrete mixture environment Ca 2+ The concentration is normal, which in turn promotes the improvement of cement's early strength and other properties. On this basis, calcium ions complex with polar groups in chitosan to form coordinated covalent bonds, which can not only improve the mechanical properties of chitosan, but also further promote the dissolution of calcium ions, making the calcium ion concentration in the early liquid phase reaction significantly increased. In addition, the radius of chitosan particles is larger than that of calcium ions, making it easier to generate smaller complexes with a coordination number of 6. Under the induction of the template effect, CO3 2- Rapidly with Ca 2+Combined to form calcite-type calcium carbonate (coordination number 6), thereby inducing the massive formation of calcite. Moreover, the addition of chitosan allows the lithium salt solid waste powder to be tightly combined with the hydration product CSH gel, which will further improve the material's ability to resist degradation. In addition, in view of the characteristics of the loose and porous surface, large specific surface area, and easy agglomeration of lithium salt solid waste powder, the addition of the composite activator and the mechanical grinding can make the composite activator particles adhere to the surface of the lithium salt solid waste or enter its internal voids, and tightly combine with the lithium salt solid waste particles, thereby improving the surface structure of the lithium salt solid waste powder, solving the problem of easy agglomeration of lithium salt solid waste, and optimizing the combination of lithium salt solid waste powder and cement. During the cement hydration process, hydration products such as calcite preferentially grow on the surface or voids of composite activator particles, which is not only conducive to the expulsion of air inside the voids of lithium salt solid waste, improving the problem of bubbles existing inside the ultra-high performance concrete matrix and difficulty in expelling bubbles due to the difficulty in filling lithium salt solid waste, but also further strengthens the bonding between lithium salt solid waste and hydration products, which helps to improve the strength performance and stability of lithium salt solid waste-based ultra-high performance concrete (UHPC).
[0040] This embodiment can effectively stimulate the activity of lithium salt solid waste volcanic ash through mechanical-chemical composite activation, and can replace silica ash and fly ash to prepare ultra-high performance concrete, effectively reduce the production cost of ultra-high performance concrete, and realize green and low-carbon solid waste resource utilization.
[0041] The chemical components of the lithium salt solid waste in this embodiment include: 70-75% SiO2, 20-25% Al2O3, 0.05-0.4% CaO, and 0.01%-5% impurity oxides, wherein the impurity oxides are a combination of one or more oxides of Fe2O3, K2O, and MgO.
[0042] Based on the same inventive concept, this embodiment also provides a method for preparing ultra-high performance concrete using activated lithium salt solid waste, comprising:
[0043] In parts by weight, 625 to 700 parts of cement, 65 to 110 parts of fly ash, 70 to 140 parts of silica fume, 70 to 180 parts of activated lithium salt solid waste, 900 to 1000 parts of quartz sand, 155 to 175 parts of water, and 10 to 17 parts of a water reducing agent are stirred and mixed to obtain a mixed material; the activated lithium salt solid waste is the activated lithium salt solid waste for ultra-high performance concrete;
[0044] 50-100 weight of steel fibers are added to the mixture and stirred evenly before pouring and forming. After curing to a specified age, ultra-high performance concrete using activated lithium salt solid waste is obtained.
[0045] Example 2
[0046] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0047] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0048] The mix ratio of ultra-high performance concrete is: PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 , the average particle size of A component activated lithium salt solid waste is 3.28μm 175.5kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 The mass ratio of the raw materials in component A is 30:24:45:1: triethanolamine: sodium sulfate: sodium silicate: grinding aid.
[0049] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0050] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0051] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0052] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0053] Example 3
[0054] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0055] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0056] PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 , the average particle size of B component activated lithium salt solid waste is 3.28μm 175.5kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 The mass ratio of the raw materials in component B is 19:25:55:1:calcium formate:calcium nitrate:chitosan:grinding aid.
[0057] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0058] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0059] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0060] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0061] Example 4
[0062] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0063] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0064] PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 , the average particle size of A component activated lithium salt solid waste is 175.5kg / m 3, 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 The mass ratio of the raw materials in component A is 30:24:45:1: triethanolamine: sodium sulfate: sodium silicate: grinding aid.
[0065] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0066] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0067] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0068] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0069] Example 5
[0070] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0071] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0072] PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 , the average particle size of B component activated lithium salt solid waste is 175.5kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3The mass ratio of the raw materials in component B is 19:25:55:1:calcium formate:calcium nitrate:chitosan:grinding aid.
[0073] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0074] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0075] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0076] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0077] Example 6
[0078] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0079] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0080] PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 AB mixed activated lithium salt solid waste with an average particle size of 3.28μm 175.5kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 The mass ratio of each raw material in component A is 30:24:45:1 for triethanolamine:sodium sulfate:sodium silicate:grinding aid, and the mass ratio of each raw material in component B is 19:25:55:1 for calcium formate:calcium nitrate:chitosan:grinding aid.
[0081] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0082] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0083] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0084] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0085] Example 7
[0086] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0087] The first step is to mix PO52.5 cement, fly ash, silica fume, activated lithium salt solid waste and quartz sand according to the mix ratio and pour them into the JJ-5 mortar mixer, and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0088] PO52.5 cement 691.2kg / m 3 , fly ash 67kg / m 3 , silica fume 71.1kg / m 3 AB mixed activated lithium salt solid waste with an average particle size of 1.48μm 175.5kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 The mass ratio of each raw material in component A is 30:24:45:1 for triethanolamine:sodium sulfate:sodium silicate:grinding aid, and the mass ratio of each raw material in component B is 19:25:55:1 for calcium formate:calcium nitrate:chitosan:grinding aid.
[0089] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0090] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0091] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0092] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0093] Comparison Example
[0094] The method for preparing ultra-high performance concrete using activated lithium salt solid waste comprises:
[0095] Step 1: Pour PO52.5 cement, fly ash, silica fume and quartz sand into the JJ-5 mortar mixer according to the mix ratio and stir slowly for 90 seconds; during the slow stirring process, slowly pour 70% of the water and the mixture of all the water reducers and defoamers into the mixing pot;
[0096] PO52.5 cement 691.2kg / m 3 , fly ash 182.1Kg / m 3 , silica fume 131.5Kg / m 3 , 40~80 mesh quartz sand 709.63kg / m 3 , 20-40 mesh quartz sand 202.75kg / m 3 , water 170.9kg / m 3 , water reducing agent 16.25kg / m 3 , copper-plated straight steel fiber 80kg / m 3 .
[0097] Step 2: After slow stirring for 90 seconds, let it stand for 30 seconds, add the remaining 30% of water, stir slowly for 180 seconds, and then stir quickly for 120 seconds;
[0098] Step 3: Slowly and evenly add the copper-plated straight steel fiber and stir slowly for 90 seconds;
[0099] Step 4: After stirring, pour the slurry into a mold (40×40×160mm) and form it in two layers using a single-side pouring method. Each layer of slurry is vibrated 60 times.
[0100] Step 5. After curing for 1 day at a temperature of 20°C and humidity above 90%, demould and place in standard curing. Set the curing temperature to 20±2°C and the humidity to greater than 95%. After curing to the specified age, test the compressive and flexural strength.
[0101] The flexural strength and compressive strength of the concrete test blocks in Examples 2-7 and the control example were recorded, and the relevant data are shown in Table 1:
[0102] Table 1 Flexural strength and compressive strength data of concrete test blocks in Examples 2-7 and Control Examples
[0103]
[0104] It can be seen from the above table that the compressive and flexural strengths of ultra-high performance concrete increased after the activated lithium salt solid waste was added separately, or after the activated lithium salt solid waste was mixed and ground into component A and component B, which confirms the application direction of activated lithium salt solid waste in ultra-high performance concrete. The effect of adding activated lithium salt solid waste powder with an average particle size of 1.48μm is better.
[0105] SEM was used to characterize the activated lithium salt solid waste powder with an average particle size of 1.48 μm and the unmilled lithium salt solid waste powder in Example 7, and the UHPC mixed with the activated lithium salt solid waste powder with an average particle size of 1.48 μm was also characterized.
[0106] Figure 1 This is a SEM image of activated lithium salt solid waste powder with an average particle size of 1.48 μm. Figure 1 The size distribution of activated lithium salt solid waste is more uniform and the sphericity is greatly improved, so it has a better filling effect when preparing UHPC, the internal pores are greatly destroyed, and most of the particles are ball-milled to 0-10μm.
[0107] Figure 2 This is the SEM image of untreated lithium salt solid waste powder. Figure 2 The lithium salt solid waste in the mine is unevenly distributed in size, has poor sphericity, and most of the edges and corners are sharp; there are many pores of about 1 to 3 μm inside.
[0108] Figure 3 This is the SEM image of UHPC mixed with activated lithium salt solid waste powder with an average particle size of 1.48μm. Figure 3 It can be clearly seen that the hydration products contain calcium sulfoxide (AFt) and growing blocky calcite crystals (Cal). This effectively shows that during the process of mixing and grinding with lithium salt solid waste, the early strength agent will adhere to the surface of the lithium salt solid waste or enter its internal voids. Therefore, during the cement hydration process, the hydration products will preferentially grow in these locations, which is not only conducive to the discharge of air inside the lithium salt solid waste, but also further strengthens the combination between the lithium salt solid waste and the hydration products. This optimized combination method helps to improve the performance and stability of lithium salt solid waste-based UHPC concrete.
[0109] It should be noted that in Examples 2 to 7, the specific process of mixing and grinding lithium salt solid waste powder and composite activator is as follows: the lithium salt solid waste powder and composite activator are mixed and poured into a ball mill, and the ball milling time is controlled to 60min and 120min respectively. The powder obtained after ball milling is aged for 1d to make it fully react evenly. The lithium salt solid waste powder after uniform aging is subjected to particle size analysis and test, and activated lithium salt solid waste powders with average particle sizes of 3.28μm (obtained by ball milling for 60min) and 1.48μm (obtained by ball milling for 120min) are obtained.
[0110] The above is an embodiment of the present invention. The above embodiments and the specific parameters in the embodiments are only for the purpose of clearly describing the invention verification process, and are not intended to limit the patent protection scope of the present invention. The patent protection scope of the present invention is still subject to its claims. Any equivalent structural changes made by using the contents of the description and drawings of the present invention should be included in the protection scope of the present invention.
Claims
1. An activated lithium salt solid waste for ultra-high performance concrete, characterized in that: It comprises lithium salt solid waste powder and a composite activator, wherein the lithium salt solid waste powder is a solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid; The composite activator comprises a composite formed by component A and component B, wherein: Component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid; Component B comprises a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
2. The activated lithium salt solid waste for ultra-high performance concrete according to claim 1, characterized in that: The chemical components of the lithium salt solid waste include: 70-75% SiO2, 20-25% Al2O3, 0.05-0.4% CaO, 0.01%-5% impurity oxides, and the impurity oxides are a combination of one or more oxides of Fe2O3, K2O, and MgO.
3. The activated lithium salt solid waste for ultra-high performance concrete according to claim 1, characterized in that: The mass ratio of each raw material in component A, triethanolamine: sodium sulfate: sodium silicate: grinding aid is 30:24:45:1, and the mass ratio of each raw material in component B, calcium formate: calcium nitrate: chitosan: grinding aid is 19:25:55:
1.
4. The activated lithium salt solid waste for ultra-high performance concrete according to claim 1, characterized in that: The average particle size of the activated lithium salt solid waste ranges from 1.48 μm to 3.28 μm.
5. A method for preparing activated lithium salt solid waste for ultra-high performance concrete, characterized in that: include: The solid waste powder obtained by extracting lithium resources from spodumene under pressure with nitric acid is dried to obtain lithium salt solid waste powder; The lithium salt solid waste powder and the composite activator are mixed and ground, and aged for at least 3 hours after the grinding is completed to obtain the activated lithium salt solid waste; the composite activator includes a complex formed by component A and component B, wherein: component A includes a mixture of triethanolamine, sodium sulfate, sodium silicate and a grinding aid; component B includes a mixture of calcium formate, calcium nitrate, chitosan and a grinding aid.
6. The method for preparing activated lithium salt solid waste for ultra-high performance concrete according to claim 5, characterized in that: The chemical components of the lithium salt solid waste include: 70-75% SiO2, 20-25% Al2O3, 0.05-0.4% CaO, 0.01%-5% impurity oxides, and the impurity oxides are a combination of one or more oxides of Fe2O3, K2O, and MgO.
7. The method for preparing activated lithium salt solid waste for ultra-high performance concrete according to claim 5, characterized in that: The mass ratio of each raw material in component A, triethanolamine: sodium sulfate: sodium silicate: grinding aid is 30:24:45:1, and the mass ratio of each raw material in component B, calcium formate: calcium nitrate: chitosan: grinding aid is 19:25:55:
1.
8. The method for preparing activated lithium salt solid waste for ultra-high performance concrete according to claim 5, characterized in that: The lithium salt solid waste powder and the composite activator are mixed and ground to an average particle size range of 1.48 μm to 3.28 μm, and the activated lithium salt solid waste is obtained after aging for at least 3 hours.
9. A method for preparing ultra-high performance concrete using activated lithium salt solid waste, characterized in that: include: In parts by weight, 625 to 700 parts of cement, 65 to 110 parts of fly ash, 70 to 140 parts of silica fume, 70 to 180 parts of activated lithium salt solid waste, 900 to 1000 parts of quartz sand, 155 to 175 parts of water, and 10 to 17 parts of a water reducing agent are stirred and mixed to obtain a mixed material; the activated lithium salt solid waste is the activated lithium salt solid waste for ultra-high performance concrete according to any one of claims 1 to 4; 50-100 weight of steel fibers are added to the mixture and stirred evenly before pouring and forming. After curing to a specified age, ultra-high performance concrete using activated lithium salt solid waste is obtained.
10. The method for preparing ultra-high performance concrete using activated lithium salt solid waste according to claim 10, characterized in that: The steel fiber is a copper-plated straight steel fiber with a length of 12 to 14 mm and a diameter of 0.18 to 0.23 mm. During the curing process to the specified age, the curing system is as follows: after casting and forming, it is cured for 1 day under the conditions of a temperature of 20°C and a humidity of more than 90%, and then demolded, and placed in an environment with a temperature of 20±2°C and a humidity of more than 95% for standard curing to the specified age.