Multifunctional filling material for coal mine goaf and preparation method of multifunctional filling material

By combining slag, fly ash and other materials, multifunctional filling materials are prepared, which solves the problems of surface subsidence, toxic gas leakage and spontaneous coal combustion in coal mine goaf, and achieves high fluidity and compressive strength of the material. In coal mine goaf filling project.

CN118993645APending Publication Date: 2024-11-22NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085030.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The formation of coal mine goaf leads to surface subsidence, leakage of toxic and harmful gases and spontaneous combustion of coal. The existing filling materials have single functions, poor fluidity, slow solidification speed, and poor resistance performance, which cannot effectively solve these problems.

Method used

Using a combination of slag, fly ash, cement, styrene acrylic emulsion, chlorine-free premature strength agent, silicate expansion agent, polycarboxylic acid water reducer and lithium carbonate coagulant, through grinding, mixing and stirring, etc. Steps to prepare a multifunctional filling material to improve the fluidity, compressive strength and resistivity of the material.

Benefits of technology

Effectively reduce the risk of surface subsidence, reduce the risk of toxic and harmful gas leakage and spontaneous combustion of coal, improve the fluidity and compressive strength of materials, and is suitable for filling projects in coal mine goafs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a multifunctional filling material for a coal mine goaf and a preparation method of the multifunctional filling material. The multifunctional filling material is prepared from the following components in percentage by weight: 53 to 55 percent of slag, 30 to 32 percent of fly ash, 8 to 10 percent of cement, 1.5 to 2.5 percent of styrene-acrylic emulsion, 1 to 2 percent of chloride-free early strength agent, 0.9 to 1.1 percent of silicate expanding agent, 0.6 to 1 percent of polycarboxylate superplasticizer and 0.4 to 0.6 percent of lithium carbonate coagulant. The material has the advantages that (1) the compressive strength of the material is better, and the settlement risk of a goaf can be effectively reduced; (2) the material has low permeability after being solidified, and leakage of poisonous and harmful gas is reduced to a certain extent; (3) the silicate expanding agent in the material has a certain inhibition effect on the residual coal, so that the risk of spontaneous combustion of the residual coal is reduced; and (4) the material has good fluidity, good grouting efficiency can be ensured, and the conveying cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of coal mine goaf filling materials, and in particular relates to a coal mine goaf multifunctional filling material and a preparation method thereof. Background Art

[0002] With the continuous exploitation of coal resources, the formation of goafs causes the underground coal structure to lose support, resulting in surface subsidence. Surface subsidence causes damage to surrounding buildings, roads and pipeline facilities, while causing irreversible damage to the ecological environment and threatening the lives of people. Therefore, solving the problem of goaf collapse caused by the mining of mineral resources is of great significance to promoting sustainable development and promoting social harmony and stability.

[0003] With the increase of coal mining, there are more and more problems such as leakage of toxic and harmful gases and spontaneous combustion of coal in coal mine goaf. The existing goaf filling materials in my country have single functions, and have problems such as unsatisfactory fluidity, slow solidification speed, and poor retardant performance. Therefore, facing a series of problems brought by coal mining, it is undoubted that it is important to develop a multifunctional filling material suitable for coal mine goaf problems. Summary of the invention

[0004] Based on the above analysis, the purpose of the present invention is to reduce the problems of surface subsidence, leakage of toxic and harmful gases, and spontaneous combustion of abandoned coal in coal mine goafs.

[0005] The first object of the present invention is to provide a multifunctional filling material for coal mine goaf, which is composed of the following components and weight percentages: slag: 53%-55%, fly ash: 30%-32%, cement: 8%-10%, styrene-acrylic emulsion 1.5%-2.5%, chlorine-free early strength agent 1%-2%, silicate expansion agent 0.9%-1.1%, polycarboxylic acid water reducer 0.6%-1%, and lithium carbonate coagulant 0.4%-0.6%.

[0006] Furthermore, the slag is a highly activated alkaline slag.

[0007] Furthermore, the fly ash is first-class F low-calcium fly ash with a fineness of ≤45 μm, a water requirement ratio of ≤95%, and a loss on ignition of ≤5.0%.

[0008] Furthermore, the cement is No. 42.5 ordinary Portland cement.

[0009] Furthermore, the slag, fly ash and cement are used as aggregate, fine material and binder of multifunctional filling materials for coal mine goaf.

[0010] Furthermore, the styrene acrylic emulsion is a modifier. After the styrene acrylic emulsion is mixed with the material, it can reduce the interfacial tension between the materials and form a polymer film on the surface of the material, thereby reducing the permeability of the material and improving the strength of the material.

[0011] Furthermore, the main components of the chlorine-free early strength agent are Na2SO4 and CaSO4, which can improve the early strength of the material and shorten the curing time of the material by promoting cement hydration reaction, reducing porosity, and preventing the precipitation of cement particles.

[0012] Furthermore, the main components of the silicate expansion agent are CaO, Fe2O3, SiO2, Al2O3, and MgO, and the hydration product after the expansion agent is mixed with the material can reduce the permeability of the material.

[0013] Furthermore, the main components of the polycarboxylate water-reducing agent include polycarboxylic acid polymers, surfactants and additives. The polycarboxylate water-reducing agent effectively reduces the water-cement ratio in the material and improves the fluidity of the material through mechanisms such as surface adsorption, water repellency, hydration inhibition and dispersion, thereby improving the strength and durability of the material.

[0014] Furthermore, the main component of the lithium carbonate coagulant is Li2CO3. The lithium carbonate coagulant can accelerate the hydration reaction of cement, promote the coagulation and hardening process of the material, and thus improve the early strength of the material through mechanisms such as ion effect, catalysis, inhibitor effect and surface tension regulation.

[0015] The second object of the present invention is to provide a method for preparing the above-mentioned multifunctional filling material for coal mine goaf, comprising the following steps:

[0016] Step 1: Put the slag into a grinding mill for grinding. The speed of the grinding mill is 2800r / min. The output fineness is below 15mm. After grinding, the slag with a particle size of 5-10mm is selected through a sieve.

[0017] Step 2, according to weight percentage, weigh 53%-55% of slag, 30%-32% of fly ash, 8%-10% of cement, 1.5%-2.5% of styrene-acrylic emulsion, 1%-2% of chlorine-free early strength agent, 0.9%-1.1% of silicate expansion agent, 0.6%-1% of polycarboxylic acid water reducer, and 0.4%-0.6% of lithium carbonate coagulant, mix the dry materials evenly and place them in a mixer, select a water-cement ratio of 0.2-0.3, pour water into the mixer and stir evenly to obtain a multifunctional filling material for coal mine goaf.

[0018] The multifunctional filling material for coal mine goaf provided by the present invention has the characteristics of simple formula, convenient construction, good compressive strength, moderate fluidity, low permeability and certain chemical resistance effect, and is suitable for promoting the filling project of coal mine goaf. Therefore, this multifunctional filling material has broad application prospects in coal mine goaf filling projects. DETAILED DESCRIPTION

[0019] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, a detailed description is given below through specific implementation methods, but the examples given are not intended to limit the present invention.

[0020] Example 1

[0021] A multifunctional filling material for coal mine goaf, mainly prepared from the following components in percentage by weight:

[0022] Slag 54%, fly ash 31%, cement 10%, styrene acrylic emulsion 1.8%, chlorine-free early strength agent 1.2%, silicate expansion agent 0.9%, polycarboxylic acid water reducer 0.7%, lithium carbonate accelerator 0.4%.

[0023] The specific preparation method is as follows:

[0024] Step 1: Put the slag into a grinding mill for grinding. The speed of the grinding mill is 2800r / min. The output fineness is below 15mm. After grinding, the slag with a particle size of 5-10mm is selected through a sieve.

[0025] Step 2, according to weight percentage, weigh 54% slag, 31% fly ash, 10% cement, 1.8% styrene acrylic emulsion, 1.2% chlorine-free early strength agent, 0.9% silicate expansion agent, 0.7% polycarboxylic acid water reducer, and 0.4% lithium carbonate coagulant, mix the dry materials evenly and place them in a mixer, select a water-cement ratio of 0.25, pour water into the mixer and stir evenly to obtain a multifunctional filling material for coal mine goaf.

[0026] The specific implementation process is as follows:

[0027] Step 1: Pour the configured multifunctional filling material for coal mine goaf into a truncated cone round mold, place it on the acrylic plate on the vibration table, lift the round mold vertically and turn on the vibrating screen. After vibrating for 30 seconds, measure the maximum diameter of the filling slurry and the diameter perpendicular to the maximum diameter. Take the average of the two diameters as the fluidity of the slurry and record the fluidity of the slurry.

[0028] Step 2, pour the remaining multifunctional filling material of the coal mine goaf into the mold pre-coated with a release agent, place the mold on a vibrating screen and vibrate it, let it stand for 24 hours and then demold it, after demolding, mark the test blocks and put them into a curing box for curing, the temperature of the curing box is 20±2℃, and the humidity is ≥95%. The test blocks are cured for 3d, 7d and 28d respectively, then taken out, and the permeability and compressive strength tests are carried out on the test blocks.

[0029] The test results are shown in Table 1:

[0030] Table 1 Test results

[0031]

[0032] Example 2

[0033] A multifunctional filling material for coal mine goaf, mainly prepared from the following components in percentage by weight:

[0034] 55% slag, 30% fly ash, 9% cement, 2% styrene acrylic emulsion, 1.5% chlorine-free early strength agent, 1% silicate expansion agent, 0.9% polycarboxylic acid water reducer, and 0.6% lithium carbonate accelerator.

[0035] The specific preparation method is as follows:

[0036] Step 1: Grind the slag into a grinding machine, and then select the slag with a particle size of 5-10 mm through a sieve.

[0037] Step 2, according to weight percentage, weigh 55% of slag, 30% of fly ash, 9% of cement, 2% of styrene-acrylic emulsion, 1.5% of chlorine-free early strength agent, 1% of silicate expansion agent, 0.9% of polycarboxylic acid water reducer, and 0.6% of lithium carbonate coagulant, mix the dry materials evenly and place them in a mixer, select a water-cement ratio of 0.25, pour water into the mixer and stir evenly to obtain a multifunctional filling material for coal mine goaf.

[0038] The specific implementation process is as follows:

[0039] Step 1: Pour the configured multifunctional filling material for coal mine goaf into a truncated cone round mold, place it on the acrylic plate on the vibration table, lift the round mold vertically and turn on the vibrating screen. After vibrating for 30 seconds, measure the maximum diameter of the filling slurry and the diameter perpendicular to the maximum diameter. Take the average of the two diameters as the fluidity of the slurry and record the fluidity of the slurry.

[0040] Step 2, pour the remaining multifunctional filling material of the coal mine goaf into the mold pre-coated with a release agent, place the mold on a vibrating screen and vibrate it, let it stand for 24 hours and then demold it, after demolding, mark the test blocks and put them into a curing box for curing, the temperature of the curing box is 20±2℃, and the humidity is ≥95%. The test blocks are cured for 3d, 7d and 28d respectively, then taken out, and the permeability and compressive strength tests are carried out on the test blocks.

[0041] The test results are shown in Table 2:

[0042] Table 2 Test results

[0043]

[0044] Example 3

[0045] A multifunctional filling material for coal mine goaf, mainly prepared from the following components in percentage by weight:

[0046] Slag 53%, fly ash 32%, cement 8%, styrene acrylic emulsion 2.3%, chlorine-free early strength agent 2%, silicate expansion agent 1.1%, polycarboxylic acid water reducer 1%, lithium carbonate accelerator 0.6%.

[0047] The specific preparation method is as follows:

[0048] Step 1: Grind the slag into a grinding machine, and then select the slag with a particle size of 5-10 mm through a sieve.

[0049] Step 2, according to weight percentage, weigh 53% slag, 32% fly ash, 8% cement, 2.3% styrene acrylic emulsion, 2% chlorine-free early strength agent, 1.1% silicate expansion agent, 1% polycarboxylic acid water reducer, and 0.6% lithium carbonate coagulant, mix the dry materials evenly and place them in a mixer, select a water-cement ratio of 0.25, pour water into the mixer and stir evenly to obtain a multifunctional filling material for coal mine goaf.

[0050] The specific implementation process is as follows:

[0051] Step 1: Pour the configured multifunctional filling material for coal mine goaf into a truncated cone round mold, place it on the acrylic plate on the vibration table, lift the round mold vertically and turn on the vibrating screen. After vibrating for 30 seconds, measure the maximum diameter of the filling slurry and the diameter perpendicular to the maximum diameter. Take the average of the two diameters as the fluidity of the slurry and record the fluidity of the slurry.

[0052] Step 2, pour the remaining multifunctional filling material of the coal mine goaf into the mold pre-coated with a release agent, place the mold on a vibrating screen and vibrate it, let it stand for 24 hours and then demold it, after demolding, mark the test blocks and put them into a curing box for curing, the temperature of the curing box is 20±2℃, and the humidity is ≥95%. The test blocks are cured for 3d, 7d and 28d respectively, then taken out, and the permeability and compressive strength tests are carried out on the test blocks.

[0053] The test results are shown in Table 3:

[0054] Table 3 Test results

[0055]

[0056] From the above results, it can be seen that the multifunctional filling materials for coal mine goaf provided by Examples 1, 2 and 3 have good compressive strength and can effectively reduce the risk of goaf settlement; the materials have low permeability after solidification, which reduces the leakage of toxic and harmful gases to a certain extent; the silicate expansion agent in the materials has a certain inhibitory effect on the coal residue, reducing the risk of spontaneous combustion of the coal residue; the materials have good fluidity, which can ensure good grouting efficiency and reduce transportation costs. All embodiments can fully meet the requirements of underground filling.

[0057] The above is a detailed introduction to a multifunctional filling material for coal mine goaf areas and a preparation method thereof provided by the present invention. The description of the embodiments used in this article is only used to help understand the method of the present invention but not to limit it, so as to facilitate the practice of the present invention by those skilled in the art. Technicians in this field can modify or replace the technical scheme of the present invention with equivalents without departing from the spirit and scope of the technical scheme of the present invention, which should be covered by the scope of the claims of the present invention.

Claims

1. A multifunctional filling material for coal mine goaf, characterized in that: It is composed of the following components and their weight percentages: 53%-55% slag, 30%-32% fly ash, 8%-10% cement, 1.5%-2.5% styrene acrylic emulsion, 1%-2% chlorine-free early strength agent, 0.9%-1.1% silicate expansion agent, 0.6%-1% polycarboxylic acid water reducer, and 0.4%-0.6% lithium carbonate accelerator.

2. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The slag is highly activated alkaline slag.

3. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The fly ash has a fineness of ≤45 μm, a water requirement ratio of ≤95%, and a loss on ignition of ≤5.0%.

4. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The styrene acrylic emulsion is a modifier.

5. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The components of the chlorine-free early strength agent include Na2SO4 and CaSO4.

6. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The components of the silicate expansion agent include CaO, Fe2O3, SiO2, Al2O3, and MgO.

7. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The components of the polycarboxylate water-reducing agent include polycarboxylic acid polymer, surfactant and auxiliary agent.

8. The multifunctional filling material for coal mine goaf according to claim 1, characterized in that: The lithium carbonate coagulant includes Li2CO3.

9. The method for preparing a multifunctional filling material for coal mine goaf according to any one of claims 1 to 8, characterized in that: Follow these steps to complete: (1) putting the slag into a grinding mill and grinding it at a speed of 2800 r / min. The discharge fineness is less than 15 mm. After grinding, the slag with a particle size of 5-10 mm is selected through a sieve; (2) Weigh each component according to the required weight percentage, mix the dry materials evenly and place them in a mixer, select the required water-cement ratio, pour water into the mixer and mix evenly to obtain a multifunctional filling material for coal mine goaf.