Ceramic-based composite material applied to mining explosion-proof lamp and preparation method of ceramic-based composite material
Through the design of ceramic matrix composite materials, combined with SiC fiber, chopped carbon fiber and graphene sheet layers, the corrosion and insufficient mechanical strength of traditional mining explosion-proof lamp materials in high temperature and high humidity environments is solved, and a higher Mechanical properties, thermal stability and corrosion resistance reduce weight and cost, providing a safer and more reliable solution for mine lighting.
Patent Information
- Application Number
- CN202411065203.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional mining explosion-proof lamp materials are prone to corrosion in high temperature and high humidity environments, have poor mechanical strength, pose safety hazards, and are large in weight that are not conducive to installation and maintenance.
Using ceramic-based composite materials, including high-purity α-Al2O3, silicon nitride, SiC fibers, chopped carbon fibers, graphene sheets and additives (such as yttrium oxide, lanthanum oxide, barium titanate and silane coupling agents), through high energy Ball milling, isostatic molding and sintering processes form composite materials with high strength, corrosion resistance and excellent thermal conductivity.
It significantly improves the tensile strength, compressive strength and fracture toughness of composite materials, enhances thermal stability and corrosion resistance, reduces the weight of lamps, reduces transportation and operation costs, extends the life of lamps, and ensures in high temperature environments. The stable operation of LED light sources and the safe operation in the electromagnetic environment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mining operating materials, in particular to a ceramic-based composite material applied to mining explosion-proof lamps and a preparation method thereof. Background Art
[0002] In the process of mining mineral resources, the mine environment is extremely complex and harsh, with factors such as high temperature, high humidity, high dust, and uncertain gas concentration. These conditions place extremely high demands on mining equipment, especially lighting systems. Traditional lighting fixtures are prone to accelerated material aging and reduced mechanical strength due to high temperatures in mine environments, or safety accidents caused by electrical failures. In particular, explosion-proof lamps must be designed not only to meet basic lighting needs, but also to ensure that they will not become ignition sources under extreme conditions. Strict requirements are placed on the flame retardancy, high temperature resistance, impact resistance, and thermal stability of the materials.
[0003] Traditional mining explosion-proof lamps are mostly made of metal materials, such as copper alloys and stainless steel. Although they have certain mechanical strength and thermal conductivity, they are prone to corrosion in high temperature and humid environments, and are heavy, which is not conducive to installation and maintenance. Therefore, it is urgent to develop a new lightweight, high-strength, high-temperature and corrosion-resistant composite material that can be used for mining explosion-proof lamps. Summary of the invention
[0004] The purpose of the present invention is to provide a ceramic-based composite material for use in mining explosion-proof lamps and a preparation method thereof. The present invention is mainly to solve the problem of poor strength and corrosion resistance of materials used in existing mining explosion-proof lamps.
[0005] To achieve the above-mentioned purpose, the technical solution of the present invention is a ceramic-based composite material for use in mining explosion-proof lamps, comprising the following raw materials in parts by weight: 60 to 65 parts of high-purity α-Al2O3, 3 to 5 parts of silicon nitride, 10 to 20 parts of SiC fibers, 3 to 5 parts of chopped carbon fibers, 1 to 3 parts of graphene sheets, and 1 to 4 parts of additives.
[0006] Preferably, the additives include yttrium oxide, lanthanum oxide, barium titanate and a silane coupling agent.
[0007] A method for preparing a ceramic-based composite material for use in mining explosion-proof lamps comprises the following steps:
[0008] S1, respectively preparing high-purity α-Al2O3, silicon nitride, graphene sheets, yttrium oxide, lanthanum oxide, barium titanate powder, and SiC fibers and chopped carbon fibers treated with a silane coupling agent;
[0009] S2. Under the protection of inert gas, weigh the above raw materials according to the weight ratio, place them in a high-energy ball mill, add an organic solvent as a dispersion medium, and ball mill for more than 24 hours to ensure that all components are evenly mixed;
[0010] S3, removing the organic solvent in the ball-milled mixture by filtering and washing, and then drying at 60° C. to 80° C. in a vacuum or low-oxygen environment until the moisture content is less than 0.5%;
[0011] S4, using isostatic pressing or injection molding technology, the dried powder is filled into a preset mold to form a preform with a certain shape and size;
[0012] S5, placing the preform in a sintering furnace protected by vacuum or inert gas, and pre-sintering at a temperature of 1400° C. to 1450° C. to promote initial densification of the powder and initial bonding of the reinforcement phase;
[0013] S6. On the basis of pre-sintering, the temperature is raised to 1700°C to 1800°C and kept at this temperature for 4 to 6 hours to complete the final densification process to ensure the complete formation of the internal structure of the composite material and the optimization of its performance;
[0014] S7. After sintering, the sintered body is slowly cooled to room temperature by gradient cooling, and the sintered body is ground and polished to meet the size and surface quality requirements of the final application.
[0015] Preferably, the organic solvent in step S2 is ethanol or isopropanol, and the rotation speed is controlled between 200 rpm and 400 rpm during ball milling to reduce fiber damage and ensure uniform mixing.
[0016] Preferably, the heating rate of the pre-sintering in step S5 does not exceed 5° C. / min.
[0017] Preferably, the pre-sintering time in step S5 is 2 to 4 hours.
[0018] The beneficial effects of the present invention are:
[0019] By adding SiC fiber, chopped carbon fiber and graphene, a three-dimensional reinforcement network is formed, which significantly enhances the tensile strength, compressive strength and fracture toughness of the composite material, enabling it to withstand frequent vibrations and impacts in mines and extend the life of the lamp;
[0020] The introduction of silicon nitride improves the thermal stability of the material, while the addition of graphene and carbon fiber optimizes thermal conductivity, helps to quickly dissipate heat, ensures that the LED light source can work efficiently and stably in a high temperature environment, reduces light decay, and improves lighting efficiency;
[0021] The addition of barium titanate and lanthanum oxide improves the dielectric properties of the material, reduces electromagnetic interference, ensures the stable operation of the lamp in a complex electromagnetic environment, and improves the safety of the system;
[0022] Compared with traditional metal materials, the composite material of the present invention significantly reduces the weight of the lamp, facilitates installation and maintenance, and reduces transportation and operation costs;
[0023] The excellent corrosion resistance of ceramic-based composite materials solves the corrosion problem of metal materials in the mine environment and prolongs the service life of lamps. At the same time, the non-toxic and environmentally friendly characteristics of the materials meet the requirements of modern safe production and sustainable development.
[0024] In summary, the present invention not only overcomes the limitations of existing mining explosion-proof lamp materials, but also demonstrates significant advantages in improving lamp performance, reducing costs, and ensuring production safety, providing important material support for the advancement of mine lighting technology. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the embodiments.
[0026] Example 1: A ceramic-based composite material for use in explosion-proof lamps for mining, comprising the following raw materials in parts by weight: 60 parts of high-purity α-Al2O3, 3 parts of silicon nitride, 10 parts of SiC fibers, 3 parts of chopped carbon fibers, 1 part of graphene sheets, and additives.
[0027] The additives include 0.25 parts of yttrium oxide, 0.25 parts of lanthanum oxide, 0.25 parts of barium titanate and 0.25 parts of a silane coupling agent.
[0028] A method for preparing a ceramic-based composite material for use in mining explosion-proof lamps comprises the following steps:
[0029] S1, respectively preparing high-purity α-Al2O3, silicon nitride, graphene sheets, yttrium oxide, lanthanum oxide, barium titanate powder, and SiC fibers and chopped carbon fibers treated with a silane coupling agent;
[0030] S2. Under the protection of inert gas, weigh the above raw materials according to the weight ratio, put them into a high-energy ball mill, add an organic solvent as a dispersion medium, and the organic solvent is ethanol. Ball mill for more than 24 hours to ensure that all components are evenly mixed. During the ball milling process, the rotation speed is controlled between 200 rpm and 400 rpm to reduce fiber damage and ensure uniform mixing;
[0031] S3, removing the organic solvent in the ball-milled mixture by filtering and washing, and then drying at 60° C. to 80° C. in a vacuum or low-oxygen environment until the moisture content is less than 0.5%;
[0032] S4, using isostatic pressing technology, filling the dried powder into a preset mold to form a preform with a certain shape and size;
[0033] S5. placing the preform in a vacuum or inert gas protected sintering furnace, and pre-sintering at a temperature of 1400° C. to 1450° C. for 2 hours. The heating rate of the pre-sintering is controlled by a program and does not exceed 5° C. / min, so as to promote the initial densification of the powder and the initial bonding of the reinforcement phase.
[0034] S6. On the basis of pre-sintering, the temperature is raised to 1700°C to 1800°C and kept at this temperature for 4 to 6 hours to complete the final densification process to ensure the complete formation of the internal structure of the composite material and the optimization of its performance;
[0035] S7. After sintering, the sintered body is slowly cooled to room temperature by gradient cooling, and the sintered body is ground and polished to meet the size and surface quality requirements of the final application.
[0036] Example 2: A ceramic-based composite material for use in explosion-proof lamps for mining, comprising the following raw materials in parts by weight: 65 parts of high-purity α-Al2O3, 5 parts of silicon nitride, 20 parts of SiC fibers, 5 parts of chopped carbon fibers, 3 parts of graphene sheets, and additives.
[0037] The additives include 1 part of yttrium oxide, 1 part of lanthanum oxide, 1 part of barium titanate and 1 part of silane coupling agent.
[0038] A method for preparing a ceramic-based composite material for use in mining explosion-proof lamps comprises the following steps:
[0039] S1, respectively preparing high-purity α-Al2O3, silicon nitride, graphene sheets, yttrium oxide, lanthanum oxide, barium titanate powder, and SiC fibers and chopped carbon fibers treated with a silane coupling agent;
[0040] S2. Under the protection of inert gas, weigh the above raw materials according to the weight ratio, put them into a high-energy ball mill, add an organic solvent as a dispersion medium, the organic solvent is isopropanol, and ball mill for more than 24 hours to ensure that all components are evenly mixed. During the ball milling process, the rotation speed is controlled between 200 rpm and 400 rpm to reduce fiber damage and ensure uniform mixing;
[0041] S3, removing the organic solvent in the ball-milled mixture by filtering and washing, and then drying at 60° C. to 80° C. in a vacuum or low-oxygen environment until the moisture content is less than 0.5%;
[0042] S4, using injection molding technology, filling the dried powder into a preset mold to form a preform with a certain shape and size;
[0043] S5. placing the preform in a vacuum or inert gas protected sintering furnace, and pre-sintering at a temperature of 1400° C. to 1450° C. for 4 hours, with a heating rate of no more than 5° C. / min, to promote the initial densification of the powder and the initial bonding of the reinforcement phase;
[0044] S6. On the basis of pre-sintering, the temperature is raised to 1700°C to 1800°C and kept at this temperature for 4 to 6 hours to complete the final densification process to ensure the complete formation of the internal structure of the composite material and the optimization of its performance;
[0045] S7. After sintering, the sintered body is slowly cooled to room temperature by gradient cooling, and the sintered body is ground and polished to meet the size and surface quality requirements of the final application.
[0046] Experimental description: According to the formula and preparation method of the present invention, a composite material sample A was prepared. At the same time, for comparative analysis, a metal material commonly used in the market, aluminum alloy, was selected as sample B as a control group;
[0047] The following key performance tests were performed on the above two samples:
[0048] Mechanical property test: three-point bending test was used to measure the bending strength, and drop hammer impact test was used to evaluate the impact resistance;
[0049] Thermal stability test: After continuous heating at high temperature (300℃ to 800℃) for a certain period of time, measure the dimensional change rate and mechanical property changes of the sample;
[0050] Corrosion resistance test: Place the sample in a salt spray chamber that simulates the mine environment. After continuous exposure for a period of time, observe the surface corrosion.
[0051] Mechanical property test results: Sample A (composite material of the present invention): flexural strength is 500 MPa, and drop weight impact energy absorption value is 30 J.
[0052] Sample B (aluminum alloy): flexural strength is 250 MPa, and drop weight impact energy absorption value is 10 J.
[0053] Thermal stability test results: After continuous heating at 800°C for 24 hours, the dimensional change rate of sample A was less than 0.3%, and the mechanical property retention rate exceeded 90%; the dimensional change rate of sample B was 1.2%, and the mechanical property retention rate was 60%.
[0054] Corrosion resistance test results: After 48 hours of salt spray corrosion test, there was almost no obvious corrosion mark on the surface of sample A, and the corrosion rate was <0.05mm / a; obvious corrosion spots appeared on the surface of sample B, and the corrosion rate was 0.2mm / a.
[0055] Comparative analysis: Sample A exhibits significantly better flexural strength and impact resistance than traditional metal materials and common ceramic-based composites, indicating that the reinforcement phase and formula optimization of the present invention effectively improve the comprehensive mechanical properties of the material and are more suitable for use in complex mine environments.
[0056] Under high temperature conditions, the composite material of the present invention exhibits smaller dimensional changes and higher performance retention rates, which proves the stability and reliability of the material in high temperature environments and is beneficial to the long-term stable operation of the lamp.
[0057] The excellent corrosion resistance of sample A reduces the erosion of lamp materials by the humid and corrosive gas environment in the mine, prolongs the service life of the lamp and reduces maintenance costs.
[0058] In summary, experimental data show that the ceramic-based composite material of the present invention is superior to the comparative sample in terms of mechanical properties, thermal stability and corrosion resistance, providing a more ideal choice for mining explosion-proof lamps and meeting the high performance requirements of mine lighting equipment in extreme environments.
[0059] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A ceramic-based composite material for use in mining explosion-proof lamps, characterized in that: The invention comprises the following raw materials in parts by weight: 60-65 parts of high-purity alpha-Al2O3, 3-5 parts of silicon nitride, 10-20 parts of SiC fiber, 3-5 parts of short-cut carbon fiber, 1-3 parts of graphene sheet and 1-4 parts of additive.
2. The ceramic-based composite material for use in mining explosion-proof lamps according to claim 1, characterized in that: The additives include yttrium oxide, lanthanum oxide, barium titanate and a silane coupling agent.
3. A method for preparing a ceramic-based composite material for use in explosion-proof lamps for use in mines, based on the ceramic-based composite material for use in explosion-proof lamps for use in mines according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1, respectively preparing high-purity α-Al2O3, silicon nitride, graphene sheets, yttrium oxide, lanthanum oxide, barium titanate powder, and SiC fiber and chopped carbon fiber treated with a silane coupling agent; S2. Under the protection of inert gas, weigh the above raw materials according to the weight ratio, place them in a high-energy ball mill, add an organic solvent as a dispersion medium, and ball mill for more than 24 hours to ensure that all components are evenly mixed; S3, removing the organic solvent in the ball-milled mixture by filtering and washing, and then drying at 60° C. to 80° C. in a vacuum or low-oxygen environment until the moisture content is less than 0.5%; S4, using isostatic pressing or injection molding technology, the dried powder is filled into a preset mold to form a preform with a certain shape and size; S5, placing the preform in a sintering furnace protected by vacuum or inert gas, and pre-sintering at a temperature of 1400° C. to 1450° C. to promote initial densification of the powder and initial bonding of the reinforcement phase; S6. On the basis of pre-sintering, the temperature is raised to 1700°C to 1800°C and kept at this temperature for 4 to 6 hours to complete the final densification process to ensure the complete formation of the internal structure of the composite material and the optimization of its performance; S7. After sintering, the sintered body is slowly cooled to room temperature by gradient cooling, and the sintered body is ground and polished to meet the size and surface quality requirements of the final application.
4. The method for preparing a ceramic-based composite material for use in a mining explosion-proof lamp according to claim 3, characterized in that: The organic solvent in step S2 is ethanol or isopropanol, and the rotation speed is controlled between 200 rpm and 400 rpm during ball milling to reduce fiber damage and ensure uniform mixing.
5. The method for preparing a ceramic-based composite material for use in a mining explosion-proof lamp according to claim 3, characterized in that: The heating rate of the pre-sintering in step S5 does not exceed 5°C / min.
6. The method for preparing a ceramic-based composite material for use in a mining explosion-proof lamp according to claim 3, characterized in that: The pre-sintering time in step S5 is 2 to 4 hours.