Zirconium-based tungstic acid, preparation method and application of zirconium-based tungstic acid in catalytic oxidation of aniline

Through the combination of zirconium-based tungsten polyacid catalyst and hydrogen peroxide, the problem of increasing cost and complexity of precious metal catalysts in the prior art is solved, and the effect of high selectivity of oxidizing aniline to azobenzene oxide is achieved, reducing the catalytic reaction and maintain the specificity and stability of the catalyst.

CN118993905AActive Publication Date: 2024-11-22NANTONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411099647.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The use of precious metal catalysts and alkaline additives in existing aniline oxidation catalytic systems increases the cost and complexity, making it difficult to achieve the production of highly selective azobenzene.

Method used

Using zirconium-based tungsten polyacid as a catalyst, the selection of aniline is achieved by reacting with zirconium oxychloride tetrahydrate, tetramethylammonium chloride and potassium chloride in sodium acetate-acetic acid buffer solution, combined with hydrogen peroxide for catalyzing. Oxidation is azobenzene oxide.

Benefits of technology

There is no need for precious metal catalysts, the cost is reduced, the catalytic reaction selectivity reaches 98.8%, and the catalyst's specificity and stability are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993905A_ABST
    Figure CN118993905A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional crystalline materials, and particularly relates to zirconium-based tungsten polyacid, a preparation method and application of the zirconium-based tungsten polyacid in catalytic oxidation of aniline. The structural formula of the zirconium-based tungsten polyacid provided by the invention is [(CH3) 4N] 3K [(PW9O32) 2 (Zr3O3)]. 45H2O, and crystallographic data and structural parameters are # imgabs0 # and # imgabs1 #, alpha is equal to 90 degrees, beta is equal to 90 degrees, and gamma is equal to 120 degrees. The zirconium-based tungsten polyacid is prepared from Na9 [PW9O34]. 7H2O as a polyacid precursor, aniline can be oxidized into azobenzene oxide by catalyzing hydrogen peroxide, the cost is low, and the selectivity is very high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional crystalline materials, and specifically relates to a zirconium-based tungsten polyacid, a preparation method and application thereof in catalyzing aniline oxidation. Background Art

[0002] Catalysis plays a very important role in the national economy. It has created huge economic and social benefits in the oil refining, chemical, environmental protection, pharmaceutical, energy, materials and other industries. Aniline is one of the most important amine substances. It is mainly used to make dyes, drugs, resins, and can also be used as a rubber vulcanization accelerator. However, there is often a large amount of aniline in the industrial wastewater of these industries, and improper treatment of aniline will cause serious environmental problems. The selective oxidation of aniline to high-value-added chemicals such as azobenzene, azobenzene oxide and nitrosobenzene using catalytic oxidation technology meets the needs of green and sustainable development. At present, aniline oxidation mainly uses Au / TiO2, Au / CeO2, RuO2 / Cu2O, Ag / C-KOH, Au1Pd1@Cx-KOH, Zr(OH)4 and other catalytic systems. However, the additional input of precious metal catalysts and alkaline additives undoubtedly increases the cost and complexity of the catalytic reaction. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a zirconium-based tungsten polyacid, a preparation method and its use in catalyzing aniline oxidation, which catalyst replaces the precious metal catalyst in the current aniline oxidation process and oxidizes aniline to oxyazobenzene with a selectivity of 98.8%.

[0004] The first aspect of the present invention provides a zirconium-based tungsten polyacid, wherein the structural formula of the zirconium-based tungsten polyacid is [(CH3)4N]3K[(PW9O 32 )2(Zr3O3)]·45H2O, the crystallographic data and structural parameters are α=90°, β=90°, γ=120°.

[0005] The second aspect of the present invention provides a preparation method of the above-mentioned zirconium-based tungsten polyacid, wherein the preparation method comprises: dissolving a polyacid precursor in a sodium acetate-acetic acid buffer solution, stirring until completely dissolved, adding zirconium oxychloride tetrahydrate, tetramethylammonium chloride, potassium chloride, and sodium carbonate, stirring to obtain a mixed solution, reacting at a constant temperature of 150-180° C. for 10-16 hours, cooling to room temperature, filtering, and producing crystals in the precipitate, repeatedly washing the crystals with the obtained filtrate, and finally obtaining pure colorless crystals, namely the zirconium-based tungsten polyacid; the polyacid precursor is Na9[PW9O 34 ]·7H2O.

[0006] Furthermore, the pH of the sodium acetate-acetic acid buffer solution is 4-5.

[0007] Furthermore, the usage ratio of the polyacid precursor, sodium acetate-acetic acid buffer solution, zirconium oxychloride tetrahydrate, tetramethylammonium chloride, potassium chloride and sodium carbonate is (1-3) g:10 mL:(1-3) g:(1-3) g:(1-3) g:(1-3) g:(1-3) g.

[0008] The third aspect of the present invention provides a use of the above-mentioned zirconium-based tungsten polyacid or the zirconium-based tungsten polyacid prepared by the above-mentioned preparation method in catalyzing the oxidation of aniline.

[0009] Furthermore, the method for catalyzing the oxidation of aniline is specifically as follows: adding the zirconium-based tungsten polyacid and hydrogen peroxide to a solution containing aniline, and reacting for 10-20 hours at a temperature of 30° C.-100° C.

[0010] In a fourth aspect of the present invention, an aniline oxidation catalyst is provided, which comprises hydrogen peroxide and zirconium-based tungsten polyacid, wherein the zirconium-based tungsten polyacid is the above-mentioned zirconium-based tungsten polyacid or the zirconium-based tungsten polyacid prepared by the above-mentioned preparation method.

[0011] Furthermore, in the aniline oxidation catalyst, the concentration of hydrogen peroxide is 30wt%, and the usage ratio of hydrogen peroxide to zirconium-based tungsten polyacid is 0.61mL: (0.028-0.065)g.

[0012] The fifth aspect of the present invention also provides a method for treating industrial wastewater, wherein the industrial wastewater contains aniline, and the method for treating industrial wastewater is specifically as follows:

[0013] The zirconium-based tungsten polyacid and hydrogen peroxide are added into industrial wastewater and reacted for 10-20 hours at a temperature of 30° C.-100° C.

[0014] Furthermore, the industrial wastewater treatment method is specifically as follows: adding the zirconium-based tungsten polyacid and hydrogen peroxide into industrial wastewater, and reacting at a temperature of 80° C. for 14 hours.

[0015] Furthermore, the concentration of the hydrogen peroxide is 30 wt %, and the usage ratio of the hydrogen peroxide to the zirconium-based tungsten polyacid is 0.61 mL: (0.028-0.065) g.

[0016] Furthermore, the concentration of the hydrogen peroxide is 30 wt %, and the usage ratio of the hydrogen peroxide to the zirconium-based tungsten polyacid is 0.61 mL: 0.037 g.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] First, the catalytic reaction does not require the addition of precious metal catalysts, which reduces costs; second, aniline is oxidized to oxyazobenzene with a selectivity of 98.8%, which is very high and the catalyst is specific. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] These and / or other aspects and advantages of the present invention will become apparent and readily understood from the following description of the preferred embodiments in conjunction with the accompanying drawings, in which:

[0020] Figure 1 This is the infrared spectrum of the compound prepared in Example 1 of the present invention;

[0021] Figure 2 is the anion structure diagram of the compound prepared in Example 1 of the present invention;

[0022] Figure 3 The results of catalytic aniline oxidation by the crystal obtained in Example 1 under different reaction times, different temperatures and different catalyst dosages;

[0023] Figure 4 Gas phase mass spectrometry results and the attribution of their peaks;

[0024] Figure 5 Infrared spectra of the compounds before and after catalysis. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] The hydrogen peroxide in the following examples is commercially available 30 wt% hydrogen peroxide.

[0027] Example 1

[0028] (1) Prepare 0.1 mol / L sodium acetate-acetic acid buffer solution with a pH of 4.

[0029] (2) Weigh 0.5 g of polyacid precursor Na9[PW9O 34 ]·7H2O is dissolved in 10mL of the above buffer solution and stirred until completely dissolved

[0030] (3) 0.13 g zirconium oxychloride tetrahydrate, 0.15 g tetramethylammonium chloride, 0.15 g potassium chloride and 0.11 g ammonium chloride were added to the above solution in sequence and stirred for 1 hour.

[0031] (4) The above mixture was placed in a polytetrafluoroethylene container, covered with a shell, and placed in an oven, the temperature was set to 180°C, and the temperature was kept for 12 hours.

[0032] (5) After the solution was cooled to room temperature, it was filtered and repeatedly washed with the filtrate to finally obtain colorless crystals with a yield of 25% (based on Na9[PW9O 34 ]·7H2O).

[0033] Example 2

[0034] (1) Prepare 0.1 mol / L sodium acetate-acetic acid buffer solution with a pH of 4.5.

[0035] (2) Weigh 0.13 g of polyacid precursor Na9[PW9O 34 ]·7H2O is dissolved in 10mL of the above buffer solution and stirred until completely dissolved.

[0036] (3) 0.13 g zirconium oxychloride tetrahydrate, 0.15 g tetramethylammonium chloride, 0.15 g potassium chloride and 0.11 g ammonium chloride were added to the above solution in sequence and stirred for 1 hour.

[0037] (4) The above mixture was placed in a polytetrafluoroethylene container, covered with a shell, and placed in an oven, the temperature was set to 180°C, and the temperature was kept for 12 hours.

[0038] (5) After the solution was cooled to room temperature, it was filtered and repeatedly washed with the filtrate to finally obtain colorless crystals with a yield of 45% (based on Na9[PW9O 34 ]·7H2O).

[0039] Example 3

[0040] (1) Prepare 0.1 mol / L sodium acetate-acetic acid buffer solution with a pH of 5.

[0041] (2) Weigh 0.13 g of polyacid precursor Na9[PW9O 34 ]·7H2O is dissolved in 10mL of the above buffer solution and stirred until completely dissolved

[0042] (3) 0.13 g zirconium oxychloride tetrahydrate, 0.15 g tetramethylammonium chloride, 0.15 g potassium chloride and 0.11 g ammonium chloride were added to the above solution in sequence and stirred for 1 hour.

[0043] (4) The above mixture was placed in a polytetrafluoroethylene container, covered with a shell, and placed in an oven, the temperature was set to 180°C, and the temperature was kept for 12 hours.

[0044] (5) After the solution was cooled to room temperature, it was filtered and repeatedly washed with the filtrate to finally obtain colorless crystals with a yield of 30% (based on Na9[PW9O 34 ]·7H2O)

[0045] Test Example 1

[0046] High-quality single crystals were selected from the crystals prepared in Example 1, Example 2, and Example 3 for structural determination, as follows: the single crystals were tested at 296 K using a Bruker APEX-IICCD and at 150 K using a Bruker D8 VENTUREPHOTON II single crystal diffractometer and all diffraction data were collected, with the radiation source being Mo Kα rays from a graphite monochromator. The coordinates of hydrogen atoms on the water molecule were obtained by difference Fourier synthesis, and the coordinates of all non-hydrogen atoms were obtained by direct method and optimized by anisotropic thermal parameters and matrix least squares method, and hydrogen atoms were directly added to the molecular formula.

[0047] The crystallographic data and structural parameters are shown in Table 1.

[0048] Table 1

[0049]

[0050] The crystal data obtained in Examples 1-3 are the same, indicating that they are the same substance, but the yields of the three methods are different.

[0051] Test Example 2

[0052] The crystals obtained in Example 1 were tested by infrared spectroscopy, and the results were as follows: Figure 1 As shown, at 964cm -1 The peak at 525 cm is attributed to W=O stretching vibration. -1 , 698cm -1 , 708cm -1 , 770cm -1 , 892cm -1 The peak at 1025 cm is attributed to WOW stretching vibration, while the peak at 1025 cm -1 , 1086cm -1 The peak at 3463cm is caused by PO stretching vibration. -1 The peak at is attributed to OH stretching vibration. The obtained compound structural formula is:

[0053] [(CH3)4N]3K[(PW9O 32 )2(Zr3O3)]·45H2O, the structure of the obtained compound is as follows Figure 2 shown.

[0054] Test Example 3

[0055] The catalytic oxidation properties of the compounds were studied with aniline as substrate, hydrogen peroxide as oxidant and water as solvent.

[0056] 0.18mL aniline, 6mL water, 0.61mL hydrogen peroxide and 0.037g compound were added to the parallel reactor, and the catalytic performance of the compound in catalyzing aniline oxidation was studied at different temperatures and reaction times. The effect of catalytic temperature and time on the amount of catalytic products was investigated based on the UV spectrum of the oily solution after the reaction. As the temperature increased (from room temperature to 80°C), the peak intensity of the solution at 310nm gradually increased, and at 80°C, the absorption peak intensity was the largest; at 80°C, as the reaction time increased, the intensity gradually increased. Therefore, it can be considered that the catalytic reaction was most thorough at 80°C for 14h ( Figure 3 a).

[0057] After determining the best time and temperature, the amount of catalyst was changed to 0.028g, 0.037g, 0.047g, 0.056g, and 0.065g. The red oil droplet was taken from the bottom layer and dissolved in methanol. The liquid UV of each sample was diluted in equal proportions. Figure 3 The results show that the best catalytic effect is obtained when the amount of catalyst is 0.037 g.

[0058] Under the optimal conditions, the oily substance after the catalytic reaction was extracted with 5 mL of methanol and tested in a gas mass spectrometer, and its concentration was 39.1 g / L. The oxidation product was mainly azobenzene oxide ( Figure 4 ), and a small amount of nitrobenzene. The selectivity of aniline oxidation to azoxybenzene is calculated to be 98.8%.

[0059] In order to compare the effects of hydrogen peroxide and catalyst on the reaction system, two groups of comparative experiments were set up. Under the optimal temperature and time conditions, when hydrogen peroxide was not added, there was almost no red oil droplets in the obtained product, indicating that the reaction basically did not occur; when no catalyst was added under the same conditions, there was a small amount of red oil droplets in the obtained product. After detection by gas chromatography-mass spectrometry, the content of azobenzene oxide was 25.2g / L. The conversion rate of aniline oxidation to azobenzene oxide was calculated to be 63.5%. The results show that the catalyst has an excellent catalytic effect on the reaction process of selective oxidation of aniline to azobenzene oxide.

[0060] In order to verify the stability of the compound during the catalytic process, the catalyzed compound was subjected to infrared spectroscopy test, such as Figure 5 As shown, the infrared spectra of the compound before and after catalysis are almost the same, indicating that the catalyst did not undergo structural changes during the catalytic process.

[0061] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A zirconium-based tungsten polyacid, characterized in that: The structural formula of the zirconium-based tungsten polyacid is [(CH3)4N]3K[(PW9O 32 )2(Zr3O3)]·45H2O, the crystallographic data and structural parameters are α=90°, β=90°, γ=120°.

2. A method for preparing the zirconium-based tungsten polyacid according to claim 1, characterized in that: The preparation method comprises: dissolving a polyacid precursor in a sodium acetate-acetic acid buffer solution, stirring until completely dissolved, adding zirconium oxychloride tetrahydrate, tetramethylammonium chloride, potassium chloride and sodium carbonate, stirring to obtain a mixed solution, reacting at a constant temperature of 150-180° C. for 10-16 hours, cooling to room temperature, filtering, and producing crystals in the precipitate, repeatedly washing the crystals with the obtained filtrate, and finally obtaining pure colorless crystals, namely the zirconium-based tungsten polyacid; the polyacid precursor is Na9[PW9O 34 ]·7H2O.

3. The preparation method according to claim 2, characterized in that: The pH of the sodium acetate-acetic acid buffer solution is 4-5.

4. The preparation method according to claim 3, characterized in that: The dosage ratio of the polyacid precursor, sodium acetate-acetic acid buffer solution, zirconium oxychloride tetrahydrate, tetramethylammonium chloride, potassium chloride and sodium carbonate is (1-3) g:10 mL: (1-3) g: (1-3) g: (1-3) g: (1-3) g: (1-3) g.

5. Use of the zirconium-based tungsten polyacid according to claim 1 or the zirconium-based tungsten polyacid prepared by the preparation method according to any one of claims 2 to 4 in catalyzing the oxidation of aniline.

6. The use according to claim 5, characterized in that: The method for catalyzing aniline oxidation is specifically as follows: adding the zirconium-based tungsten polyacid and hydrogen peroxide into a solution containing aniline, and reacting for 10-20 hours at a temperature of 30° C.-100° C.

7. An aniline oxidation catalyst, characterized in that The aniline oxidation catalyst comprises hydrogen peroxide and zirconium-based tungsten polyacid, and the zirconium-based tungsten polyacid is the zirconium-based tungsten polyacid according to claim 1 or the zirconium-based tungsten polyacid prepared by the preparation method according to any one of claims 2-4.

8. The aniline oxidation catalyst according to claim 7, characterized in that: In the aniline oxidation catalyst, the concentration of the hydrogen peroxide is 30wt%, and the usage ratio of the hydrogen peroxide to the zirconium-based tungsten polyacid is 0.61mL:(0.028-0.065)g.

9. A method for treating industrial wastewater containing aniline, characterized in that: The industrial wastewater treatment method is specifically: The zirconium-based tungsten polyacid and hydrogen peroxide are added into industrial wastewater and reacted for 10-20 hours at a temperature of 30° C.-100° C.

10. The industrial wastewater treatment method according to claim 9, characterized in that: The concentration of the hydrogen peroxide is 30 wt %, and the usage ratio of the hydrogen peroxide to the zirconium-based tungsten polyacid is 0.61 mL: (0.028-0.065) g.

Citation Information

Patent Citations

  • Germanium tungstate with efficient Lewis acid-base synergistic catalytic performance

    CN114534790A

  • Tungsten-doped polyaniline supported palladium catalyst and preparation method and application thereof

    CN114985017A

  • {P4Mo6} crystalline state-based polyacid catalyst capable of selectively oxidizing aniline under visible light condition and application of {P4Mo6} crystalline state-based polyacid catalyst

    CN116196951A

  • Application of zirconium hydroxide and copper oxide physical mixed catalyst for catalyzing aniline or derivative thereof to prepare nitrosobenzene or derivative thereof

    CN117920215A