Acrylic emulsion for spinning full-shading composite fabric, raw material composition of acrylic emulsion and preparation method of acrylic emulsion
By using a specific ratio of acrylate monomers and crosslinking monomers in a low-temperature crosslinking reaction, combined with the urethane groups of TPU film, the problem of low bonding strength of existing water-based acrylic emulsions is solved, enabling efficient production and environmentally friendly processing of full-light-blocking composite textile fabrics.
Patent Information
- Application Number
- CN202411090341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing water-based acrylic emulsions have low bonding strength when used in textile blackout composite fabrics, resulting in complicated processing procedures, high energy consumption, and significant environmental pressure.
By using a specific ratio of acrylate soft monomers, hard monomers, and crosslinking monomers, the bonding strength is improved through a low-temperature crosslinking reaction. Combined with the crosslinking reaction between the urethane groups on the TPU film and the acrylic polymer chains, the bonding strength of the composite fabric is enhanced.
It improves the adhesion between TPU film and textile fabric, simplifies the processing steps, reduces energy consumption, and enhances environmental performance.
Smart Images

Figure BDA0004986358130000061 
Figure BDA0004986358130000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile fabric preparation, and in particular relates to an acrylic emulsion for textile full-light-shielding composite fabric, a raw material composition thereof and a preparation method thereof. Background Art
[0002] Full blackout curtains are very important in modern life. Conventional full blackout curtains are made through multi-layer foam coating, but the multi-layer coating process is complicated and energy-intensive, which is not conducive to improving production efficiency. In addition, the coating process is prone to produce waste gas and wastewater, which puts great pressure on environmental protection.
[0003] Thermoplastic polyurethane (TPU) film is a polymer compound formed by the reaction of polyols and isocyanates. It has the characteristics of good toughness, good weather resistance, and can be heat processed. It is widely used in textile composite fabrics. In the textile industry, the full light-shielding effect can be achieved by replacing multiple coating processes with TPU light-shielding film, which can shorten the processing process and reduce energy consumption. At present, full light-shielding composite fabrics are usually made by bonding TPU light-shielding film to textile fabrics through adhesives such as polyurethane emulsions and water-based acrylic emulsions, and then hot pressing. However, the bonding strength of existing water-based acrylic emulsions used for composite fabrics is relatively low. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems and provide an acrylic emulsion for textile full light-shielding composite fabric, a raw material composition and a preparation method thereof. The acrylic emulsion of the present invention is used for textile full light-shielding composite fabric bonding and has strong adhesion fastness.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] In one aspect, the present invention provides a raw material composition of acrylic emulsion for textile full-shading composite fabrics, which comprises the following components in parts by weight:
[0007] 500 parts of water, 360-500 parts of soft monomer, 30-80 parts of hard monomer, 7-20 parts of first crosslinking monomer, 2-3 parts of second crosslinking monomer, 5-8 parts of emulsifier, 1-3 parts of initiator, 1-1.5 parts of redox initiator.
[0008] In some embodiments, the soft monomer includes at least one of methyl acrylate, ethyl acrylate, butyl acrylate, and isooctyl acrylate.
[0009] In some embodiments, the hard monomer includes methyl methacrylate and / or butyl methacrylate.
[0010] In some embodiments, the first cross-linking monomer and the second cross-linking monomer include at least one of acrylic acid, diacetone acrylamide, and adipic acid dihydrazide.
[0011] In some embodiments, the emulsifier is an anionic emulsifier, including at least one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium dodecyl sulfonate.
[0012] In some embodiments, the initiator includes one of sodium persulfate, potassium persulfate, and ammonium persulfate.
[0013] In some embodiments, the redox initiator includes one of tert-butyl hydroperoxide-sodium iodide and tert-butyl hydroperoxide-vitamin C.
[0014] In some embodiments, the soft monomer is selected from butyl acrylate and / or ethyl acrylate and / or isooctyl acrylate.
[0015] In some embodiments, the hard monomer is methyl methacrylate.
[0016] In some embodiments, the emulsifier is sodium lauryl sulfate.
[0017] In some embodiments, the initiator is ammonium persulfate.
[0018] In some embodiments, the redox initiator is tert-butyl hydroperoxide-vitamin C.
[0019] In some embodiments, the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric also includes 1 to 1.5 parts of a defoaming agent.
[0020] In some embodiments, the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric also includes 1 to 1.5 parts of a preservative.
[0021] In some embodiments, the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric also includes 3 to 8 parts of ammonia water.
[0022] In some embodiments, the defoaming agent is a mineral oil defoaming agent.
[0023] In some embodiments, the preservative is methylisothiazolinone.
[0024] In another aspect, the present invention provides a method for preparing an acrylic emulsion for textile full-light-shielding composite fabric, comprising the following steps:
[0025] (1) stirring and pre-emulsifying water, an emulsifier, a soft monomer, a hard monomer, and a first cross-linking monomer to obtain an emulsified monomer;
[0026] (2) adding water to the reaction kettle, starting stirring, raising the temperature to 84° C., adding part of the initiator to the reaction kettle, and after 2 to 3 minutes, adding part of the emulsified monomer for pre-reaction;
[0027] (3) After the preliminary reaction is completed, the temperature of the reactor is stabilized at 84° C., and the remaining emulsified monomer and the remaining initiator are added dropwise to the reactor. After the addition is completed, the reaction is carried out by keeping the temperature constant;
[0028] (4) After the insulation is completed, the temperature is lowered to 72-75°C, and a redox initiator is added dropwise to continue the reaction;
[0029] (5) After the reaction is completed, the temperature is lowered to 45° C., a defoamer and a preservative are added dropwise, ammonia water is added dropwise, the pH is adjusted to about 7, a second cross-linking monomer is added dropwise, and the mixture is stirred to obtain the acrylic emulsion for textile full light-shielding composite fabric.
[0030] In step (1), the weight proportion of water is 150 parts.
[0031] In step (1), the stirring time is 30 min.
[0032] In step (2), the weight proportion of water is 250 parts.
[0033] In step (2), the weight proportion of the initiator is 1 to 2 parts.
[0034] In step (2), part of the emulsified monomers is 3-4% of the total amount of the emulsified monomers.
[0035] In step (2), the pre-reaction time is 10 to 15 minutes.
[0036] In step (3), the dropping time is 3 to 4 hours.
[0037] In step (3), the insulation reaction time is 1 to 1.5 hours.
[0038] In step (4), the reaction time is 0.5 to 1.5 h.
[0039] In step (5), the stirring time is 20 min.
[0040] In step (2) and step (3), the initiator is added in the form of an aqueous solution; preferably, the initiator is dissolved in the remaining water to obtain an aqueous solution of the initiator.
[0041] The third aspect of the present invention further provides an acrylic emulsion for textile full-light-shielding composite fabrics, which is prepared by the above-mentioned preparation method of acrylic emulsion for textile full-light-shielding composite fabrics.
[0042] In some embodiments, the glass transition temperature of the acrylic emulsion used for textile full-light-shielding composite fabric is -40°C to -35°C.
[0043] The water-based acrylic emulsion prepared by the invention has a soft hand feel after drying; the pH value of the emulsion is about 7, and the neutral condition can improve the stability of the emulsion.
[0044] The positive and progressive effects of the present invention are:
[0045] The present invention copolymerizes acrylic soft monomers and hard monomers according to a suitable ratio, and then selects a suitable cross-linking monomer to introduce reactive groups ketocarbonyl and hydrazide groups that can be cross-linked at low temperatures into the polymer molecular chain. The active hydrogen on the hydrazide group can react with the ketocarbonyl group, and cross-linking occurs inside the macromolecule, giving the polymer material a certain toughness and elasticity. In addition, the carbamate on the thermoplastic polyurethane (TPU) film is a very strong reactive group, and the active hydrogen on the carbamate group can cross-link with the ketocarbonyl on the acrylic polymer macromolecule chain, directly improving the adhesion fastness between the TPU film and the acrylic emulsion. At the same time, the active hydrogen on the hydrazide group can also cross-link with the carbonyl on the carbamate, further improving the adhesion fastness between the acrylic emulsion and the TPU. In addition to the low-temperature cross-linking property, the introduction of carboxyl groups into the acrylic polymer molecular chain can cross-link with the hydroxyl on the base cloth at a higher temperature, that is, improve the fastness of the acrylic emulsion and the textile fabric, and finally achieve the purpose of enhancing the adhesion fastness of the composite fabric through secondary curing. DETAILED DESCRIPTION
[0046] The present invention is described in detail below in conjunction with the embodiments, and the technical scheme of the present invention is clearly and completely described to facilitate the understanding of the present invention by those skilled in the art. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods not mentioned in detail are process steps or preparation methods known to those skilled in the art.
[0047] Among them, anionic emulsifier: sodium lauryl sulfate, China Light Industry Group;
[0048] Initiator: ammonium persulfate, Shanghai Tianyue Chemical Co., Ltd.;
[0049] Tert-butyl hydroperoxide, Taizhou Haixiang Chemical Co., Ltd.;
[0050] N-Hydroxymethyl acrylamide, Shandong Guanchang Chemical Technology Co., Ltd.;
[0051] Glycidyl methacrylate, Shandong Hongrun Chemical Co., Ltd.;
[0052] Hydroxyethyl acrylate, Shandong Haideng New Materials Co., Ltd.
[0053] Example 1
[0054] An acrylic emulsion for textile full-light-shielding composite fabric, the raw material composition of which comprises the following components in parts by weight, as shown in Table 1.
[0055] Table 1
[0056] Specific compounds Weight parts (parts) water 500 Soft monomer: n-butyl acrylate 300 Soft monomer: ethyl acrylate 60 Soft monomer: 2-ethylhexyl acrylate 40 Hard monomer: methyl methacrylate 40 First cross-linking monomer: acrylic acid 12 First cross-linking monomer: diacetone acrylamide 4 Second cross-linking monomer: adipic acid dihydrazide 2 Emulsifier: Sodium lauryl sulfate 5 Initiator: ammonium persulfate 1 Redox initiator: tert-butyl hydroperoxide-vitamin C 1 Defoamer: Mineral oil defoamer 1 Preservative: Methylisothiazolinone 1 ammonia 8
[0057] The preparation method specifically comprises the following steps:
[0058] (1) Add 150 parts of water into an emulsifying tank, add 5 parts of sodium lauryl sulfate, 300 parts of n-butyl acrylate, 60 parts of ethyl acrylate, 40 parts of methyl methacrylate, 40 parts of isooctyl acrylate, 12 parts of acrylic acid, and 4 parts of diacetone acrylamide, and stir rapidly for pre-emulsification for 30 minutes to obtain an emulsified monomer.
[0059] (2) Add 250 parts of water to the reactor, start stirring, and heat to 84°C. Use the remaining water to dissolve the initiator for later use. Add 0.5 parts of the initiator to the reactor, add 3% of the emulsified monomer 2 minutes later, and initiate the reaction for 10 minutes.
[0060] (3) After the preliminary reaction, the temperature of the reactor was stabilized at 84°C, and the remaining emulsified monomer and initiator were added dropwise to the reactor for 3 hours. After the addition was completed, the temperature was kept constant for 1 hour.
[0061] (4) After the insulation is completed, the temperature is lowered to 72-75°C, and the redox initiator is added dropwise, and the reaction is continued for 0.5 h.
[0062] (5) After the reaction is completed, the temperature is lowered to 45° C., a defoamer and a preservative are added dropwise, ammonia water is added dropwise, the pH is adjusted to about 7, adipic acid dihydrazide that has been dissolved is added dropwise, and the mixture is stirred for 20 min to obtain a water-based acrylic emulsion.
[0063] Example 2
[0064] An acrylic emulsion for textile full-light-shielding composite fabric, the raw material composition of which comprises the following components in parts by weight, as shown in Table 2.
[0065] Table 2
[0066]
[0067]
[0068] In this embodiment, the preparation method is the same as that in Embodiment 1.
[0069] Example 3
[0070] An acrylic emulsion for textile full-light-shielding composite fabric, the raw material composition of which comprises the following components in parts by weight, as shown in Table 3.
[0071] Table 3
[0072] Specific compounds Weight parts (parts) water 500 Soft monomer: n-butyl acrylate 400 Soft monomer: ethyl acrylate 40 Soft monomer: 2-ethylhexyl acrylate 20 Hard monomer: methyl methacrylate 60 First cross-linking monomer: acrylic acid 9 First cross-linking monomer: diacetone acrylamide 6 Second cross-linking monomer: adipic acid dihydrazide 3 Emulsifier: Sodium lauryl sulfate 8 Initiator: ammonium persulfate 3 Redox initiator: tert-butyl hydroperoxide-vitamin C 1.5 Defoamer: Mineral oil defoamer 1.5 Preservative: Methylisothiazolinone 1.5 ammonia 6
[0073] In this embodiment, the preparation method is the same as that in Embodiment 1.
[0074] Comparative Example 1
[0075] The only difference from Example 1 is that 4 parts of diacetone acrylamide are replaced by 6 parts of N-methylol acrylamide, and 2 parts of adipic acid dihydrazide are replaced by 4 parts of N-methylol acrylamide.
[0076] Comparative Example 2
[0077] The only difference from Example 2 is that 5 parts of diacetone acrylamide are replaced by 6 parts of hydroxyethyl acrylate, and 2.5 parts of adipic acid dihydrazide are replaced by 4 parts of hydroxyethyl acrylate.
[0078] Comparative Example 3
[0079] The only difference from Example 3 is that 6 parts of diacetone acrylamide are replaced by 7 parts of glycidyl methacrylate, and 3 parts of adipic acid dihydrazide are replaced by 3 parts of glycidyl methacrylate.
[0080] Comparative Example 4
[0081] The only difference from Example 3 is that the weight parts of n-butyl acrylate are 180 parts, the weight parts of ethyl acrylate are 130 parts, the weight parts of acrylic acid are 18 parts, the weight parts of diacetone acrylamide are 3 parts, and the weight parts of adipic acid dihydrazide are 1.5 parts.
[0082] Comparative Example 5
[0083] The only difference from Example 3 is that the weight parts of n-butyl acrylate are 470 parts, the weight parts of ethyl acrylate are 30 parts, the weight parts of methyl methacrylate are 30 parts, the weight parts of acrylic acid are 20 parts, the weight parts of diacetone acrylamide are 2 parts, and the weight parts of adipic acid dihydrazide are 1 part.
[0084] Comparative Example 6
[0085] The raw material composition of this comparative example includes the following components in parts by weight, see Table 4.
[0086] Table 4
[0087] Specific compounds Weight parts (parts) water 500 Soft monomer: n-butyl acrylate 400 Hard monomer: methyl methacrylate 100 First cross-linking monomer: acrylic acid 15 First cross-linking monomer: diacetone acrylamide 0.25 Second cross-linking monomer: adipic acid dihydrazide 0.125 Emulsifier: Sodium lauryl sulfate 4 Emulsifier: Octylphenol polyoxyethylene (10) ether 8 Initiator: Potassium persulfate 2.25 Redox initiator: tert-butyl hydroperoxide-vitamin C 1.25 Defoamer: Mineral oil defoamer 1.25 Preservative: Methylisothiazolinone 1.25 Sodium bicarbonate 0.125
[0088] In this comparative example, the preparation method is the same as that in Example 1.
[0089] Comparative Example 7
[0090] Commercially available product, acrylic emulsion model 880 produced by Tongxiang Xingbang Technology Co., Ltd.
[0091] Product performance testing
[0092] 1. Particle size test: measured using ZEN1690 laser particle size analyzer.
[0093] 2. Washing fastness test: According to GB / T 3921-2008 Textiles - Tests for color fastness to soap washing, the emulsion is applied to the fabric and TPU laminating process, and the washing fastness test is carried out. The fastness is determined according to the degree of film degumming.
[0094] 3. Glass transition temperature: measured using DSC differential scanning calorimeter.
[0095] The performance tests were performed on the products obtained in Examples 1 to 3 and Comparative Examples 1 to 5. The specific test results are shown in Table 4.
[0096] Table 4
[0097] Sample name Particle size (nm) <![CDATA[Washing fastness grade 1 > Glass transition temperature(℃) Example 1 195 Level 4 -35 Example 2 197 Level 4.5 -37 Example 3 192 Level 5 -40 Comparative Example 1 199 Level 3 -34 Comparative Example 2 195 Level 2.5 -36 Comparative Example 3 193 Level 2.5 -35 Comparative Example 4 194 Level 3 -30 Comparative Example 5 196 Level 3 -44 Comparative Example 6 193 Level 2.5 -33 Comparative Example 7 194 Level 3.5 -37
[0098] Note: 1 The higher the washing fastness grade, the better the fastness.
[0099] As shown in Table 1, the water washing fastness of the emulsions in Example 1, Example 2, and Example 3 gradually increases. From the perspective of the synthetic formula, in the samples of Example 1, Example 2, and Example 3, the proportion of low-temperature crosslinking monomers: diacetone acrylamide and adipic acid dihydrazide gradually increases. The two can both self-crosslink inside the molecular chain at a lower temperature and crosslink with the carbamate group in TPU, giving the TPU film and the acrylic emulsion adhesive surface excellent fastness. At the same time, the acrylic acid in the sample can crosslink with the hydroxyl group in the base fabric at a higher temperature, and the combination of the two can give the composite fabric a good fit fastness.
[0100] In Comparative Examples 1, 2, and 3, the low-temperature self-crosslinking monomers are replaced with N-hydroxymethyl acrylamide, hydroxyethyl acrylate, and glycidyl methacrylate, respectively. As shown in Table 4, the washing fastness of the comparative examples is not as good as that of the samples in the examples. From the perspective of molecular structure, the functional groups in N-hydroxymethyl acrylamide, hydroxyethyl acrylate, and glycidyl methacrylate can react with the hydroxyl groups on the base fabric, but are not conducive to crosslinking with the active groups on TPU, so the composite fabric prepared has poor bonding fastness.
[0101] The results in Table 4 show that the fastness of Comparative Examples 4 and 5 is poor. The proportion of polymerized monomers is adjusted in Comparative Examples 4 and 5. In Comparative Example 4, the proportion of n-butyl acrylate and low-temperature self-crosslinking monomer is reduced, and the proportion of ethyl acrylate is increased. In Comparative Example 5, the amount of n-butyl acrylate is increased, and the proportion of ethyl acrylate, methyl methacrylate, and low-temperature self-crosslinking monomer is reduced. From the perspective of molecular structure, the side chain in n-butyl acrylate is relatively long, and intermolecular forces can be generated between the TPU polymer molecular chains in the polymer macromolecular chain, thereby improving the adhesion fastness. Comparative Example 4 reduces the proportion of n-butyl acrylate and increases the proportion of ethyl acrylate, thereby weakening the intermolecular forces between the molecular chains, and correspondingly resulting in poor adhesion fastness of the composite fabric. Comparative Example 5 increases the proportion of n-butyl acrylate, but compared with Comparative Example 4, the proportion of low-temperature self-crosslinking monomer is reduced, so the adhesion fastness of the composite fabric is not improved.
[0102] The raw material composition in Comparative Example 6 has poor fastness when used for bonding TPU light-shielding film and textile fabric, indicating that the monomer ratio and the cross-linking monomer ratio have a great influence on the application.
[0103] Comparative Example 7 is a competitive product currently on the market. By comparison, it can be seen that the adhesion of the competitive emulsion on the market is worse than that of the emulsion of the present invention, which shows that the present invention has certain technical innovations and progress.
[0104] From the above analysis, it can be seen that the bonding fastness of the water-based acrylic emulsion used for bonding TPU shading film and textile fabrics in this application is not only related to the cross-linking bond of the low-temperature self-crosslinking functional monomer, but also has an effect on the interaction between the acrylic polymer molecular chain and the TPU polymer molecular chain. Generally, the price of low-temperature self-crosslinking functional monomers is relatively high, and the synergistic effect of the cross-linking monomer and the acrylic monomer can maximize the bonding fastness of the composite fabric within a suitable cost range.
[0105] In summary, the present invention provides a method for preparing an acrylic emulsion for textile full-light-shielding composite fabrics, which is applied to the bonding of TPU light-shielding film and textile fabrics to obtain a composite fabric with good fastness. The prepared composite fabric has a soft feel and can be used for full-light-shielding soft curtains.
[0106] Finally, it should be noted that in the present invention, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements that are inherent to such process, method, article or apparatus.
[0107] Although the present disclosure has been disclosed above through the description of the specific embodiments of the present disclosure, it should be understood that those skilled in the art can design various modifications, improvements or equivalents to the present disclosure within the spirit and scope of the attached scheme. These modifications, improvements or equivalents should also be considered to be included in the scope of protection claimed by the present disclosure.
Claims
1. A raw material composition of acrylic emulsion for textile full light-shielding composite fabrics, It is characterized in that It includes the following components in parts by weight: 500 parts of water, 360-500 parts of soft monomer, 30-80 parts of hard monomer, 7-20 parts of first crosslinking monomer, 2-3 parts of second crosslinking monomer, 5-8 parts of emulsifier, 1-3 parts of initiator, 1-1.5 parts of redox initiator.
2. The raw material composition of acrylic emulsion for textile full light-shielding composite fabric according to claim 1, It is characterized in that The soft monomer includes at least one of methyl acrylate, ethyl acrylate, butyl acrylate and isooctyl acrylate; and / or, the hard monomer comprises methyl methacrylate and / or butyl methacrylate; And / or, the first cross-linking monomer and the second cross-linking monomer include at least one of acrylic acid, diacetone acrylamide, and adipic acid dihydrazide; And / or, the emulsifier is an anionic emulsifier, including at least one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium dodecyl sulfonate; And / or, the initiator includes one of sodium persulfate, potassium persulfate, and ammonium persulfate; And / or, the redox initiator includes one of tert-butyl hydroperoxide-sodium iodide and tert-butyl hydroperoxide-vitamin C.
3. The raw material composition of acrylic emulsion for textile full light-shielding composite fabric according to claim 2, It is characterized in that The soft monomer is selected from butyl acrylate and / or ethyl acrylate and / or isooctyl acrylate; and / or, the hard monomer is methyl methacrylate; And / or, the emulsifier is sodium lauryl sulfate; And / or, the initiator is ammonium persulfate; And / or, the redox initiator is tert-butyl hydroperoxide-vitamin C.
4. The raw material composition of acrylic emulsion for textile full light-shielding composite fabric according to claim 1, It is characterized in that The raw material composition of the acrylic emulsion for textile full-shading composite fabric also includes 1 to 1.5 parts of defoaming agent; And / or, the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric also includes 1 to 1.5 parts of a preservative; And / or, the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric also includes 3 to 8 parts of ammonia water.
5. The raw material composition of acrylic emulsion for textile full light-shielding composite fabric according to claim 4, It is characterized in that The defoamer is a mineral oil defoamer; And / or, the preservative is methylisothiazolinone.
6. A method for preparing an acrylic emulsion for textile full-shading composite fabrics, It is characterized in that The raw material of the acrylic emulsion for textile full-light-shielding composite fabric comprises the raw material composition of the acrylic emulsion for textile full-light-shielding composite fabric as claimed in any one of claims 1 to 5, and the method comprises the following steps: (1) stirring and pre-emulsifying water, an emulsifier, a soft monomer, a hard monomer, and a first cross-linking monomer to obtain an emulsified monomer; (2) adding water to the reaction kettle, starting stirring, raising the temperature to 84° C., adding part of the initiator to the reaction kettle, and after 2 to 3 minutes, adding part of the emulsified monomer for pre-reaction; (3) After the preliminary reaction is completed, the temperature of the reactor is stabilized at 84° C., and the remaining emulsified monomer and the remaining initiator are added dropwise to the reactor. After the addition is completed, the reaction is carried out by keeping the temperature constant; (4) After the insulation is completed, the temperature is lowered to 72-75°C, and a redox initiator is added dropwise to continue the reaction; (5) After the reaction is completed, the temperature is lowered to 45° C., a defoamer and a preservative are added dropwise, ammonia water is added dropwise, the pH is adjusted to about 7, a second cross-linking monomer is added dropwise, and the mixture is stirred to obtain the acrylic emulsion for textile full light-shielding composite fabric.
7. The method for preparing the acrylic emulsion for textile full light-shielding composite fabric according to claim 6, It is characterized in that The preparation method satisfies at least one of the following conditions: In step (1), the weight proportion of water is 150 parts; In step (1), the stirring time is 30 min; In step (2), the weight proportion of water is 250 parts; In step (2), the weight proportion of the initiator is 1 to 2 parts; In step (2), part of the emulsified monomers is 3-4% of the total amount of the emulsified monomers; In step (2), the pre-reaction time is 10 to 15 minutes; In step (3), the dripping time is 3 to 4 hours; In step (3), the insulation reaction time is 1 to 1.5 hours; In step (4), the reaction time is 0.5 to 1.5 h; In step (5), the stirring time is 20 min.
8. The method for preparing the acrylic emulsion for textile full light-shielding composite fabric according to claim 6, It is characterized in that In step (2) and step (3), the initiator is added in the form of an aqueous solution; preferably, the initiator is dissolved in the remaining water to obtain an aqueous solution of the initiator.
9. An acrylic emulsion for textile full light-shielding composite fabrics, It is characterized in that The acrylic emulsion is prepared by the method for preparing the acrylic emulsion for textile full light-shielding composite fabric according to any one of claims 6 to 8.
10. The acrylic emulsion for textile full light-shielding composite fabric according to claim 9, It is characterized in that The glass transition temperature of the acrylic emulsion is -40°C to -35°C.