Modified PMMA resin, PMMA product and preparation method thereof

Through the copolymerization and composite molding technology of methyl methacrylate and reactive silicone resin, the problems of high hydrophobic modification cost and limited adhesion are solved, and low-cost, stable hydrophobic performance and easy-to-clean effect are achieved. It is suitable for bathroom products. .

CN118994497APending Publication Date: 2024-11-22GUANGDONG LEHUA HOME FURNISHING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148798.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing PMMA hydrophobic modification technology has problems such as high cost, limited adhesion and easy falloff, and it is difficult to effectively apply in the bathroom field.

Method used

Methyl methacrylate and reactive silicone resin are used to prepare modified PMMA resin through esterification and ring opening reaction, epoxy silicone oil is added to improve hydrophobic properties, and combined with the PMMA substrate layer through composite molding process to form a stable Easy-to-clean functional layer.

Benefits of technology

It achieves low-cost, stable hydrophobic performance and easy-to-clean effect, avoids coating peeling problems, and is suitable for easy-to-clean bathtubs, star basins and other products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994497A_ABST
    Figure CN118994497A_ABST
Patent Text Reader

Abstract

The invention discloses modified PMMA (polymethyl methacrylate) resin, a PMMA product and a preparation method of the modified PMMA resin, the modified PMMA resin is obtained by copolymerizing methyl methacrylate and active organic silicon resin, and the active organic silicon resin is prepared by the following method: carrying out esterification reaction on a hydroxyl-containing allyl monomer and an anhydride compound to obtain an intermediate with monocarboxyl; and carrying out ring-opening reaction on the intermediate with the monocarboxyl and epoxy silicone oil to obtain the active organic silicon resin. The modified PMMA resin is mainly composed of the active organic silicon resin and the methyl methacrylate monomer, the methyl methacrylate monomer provides a molecular chain skeleton, the active organic silicon resin provides a hydrophobic functional branch chain anchored on the resin, so that the PMMA resin has stable and long-acting hydrophobic performance, the price of the epoxy silicone oil is low, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic glass, in particular to a modified PMMA resin, a PMMA product and a preparation method thereof. Background Art

[0002] Polymethyl methacrylate (PMMA), also known as organic glass, commonly known as acrylic, not only has good transparency, dimensional stability, mechanical properties, sound insulation, insulation and weather resistance, but also is easy to dye, easy to process, has a small specific gravity and beautiful appearance. It is often used as soundproof doors and windows, light boxes, signboards, lighting covers, instrument panels and covers, artworks, toys, etc., and is now also used in easy-to-clean bathtubs, star basins, wash basins and other products. However, since the surface of PMMA plastic plate is hydrophilic, it is easy to adsorb and deposit impurities such as dust, and has poor self-cleaning ability, which limits its application in the bathroom field. Therefore, it is of great significance to modify its surface to be hydrophobic.

[0003] At present, many technologies for hydrophobic modification of PMMA have been disclosed, but these technologies have some disadvantages to a greater or lesser extent. A related technology discloses utilizing the hydrophobic and oleophobic properties of perfluoroacrylate to copolymerize perfluoroacrylate with acrylic, so that the copolymer resin has good antifouling and stain resistance properties. However, the molecular weight of the fluorinated monomer is small, and it is difficult to form an effective hydrophobic structure. A large amount of addition is required to achieve a certain hydrophobic effect. The cost is high and it is difficult to promote and apply. Another related technology discloses coating a highly hydrophobic and stain-resistant polymethyl methacrylate coating on an organic glass substrate, so that the organic glass surface has strong hydrophobicity and stain resistance, but the adhesion of this coating to the substrate is limited, and it is easy to crack, fall off and fail. Summary of the invention

[0004] The present invention aims to solve at least one of the above technical problems in the related art to a certain extent. To this end, the present invention provides a modified PMMA resin, a PMMA product and a preparation method thereof.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] The invention provides a modified PMMA resin, wherein the modified PMMA resin is obtained by copolymerizing methyl methacrylate and an active silicone resin, and the active silicone resin is prepared by the following method: an olefin monomer containing a hydroxyl group is subjected to an esterification reaction with an acid anhydride compound to obtain an intermediate with a single carboxyl group, and then the intermediate with the single carboxyl group is subjected to a ring-opening reaction with epoxy silicone oil to obtain the active silicone resin; wherein the molecular weight of the epoxy silicone oil is 5000-500000.

[0007] Epoxy silicone oil is a polysiloxane with active epoxy groups at both ends. In the esterification reaction, the hydroxyl group in the hydroxyl-containing olefin monomer reacts with the anhydride group of the anhydride compound to obtain a monocarboxyl intermediate; in the ring-opening reaction, the carboxyl group of the intermediate reacts with the epoxy group of the epoxy silicone oil.

[0008] According to some embodiments of the present invention, the content of the reactive silicone resin in the modified PMMA resin is 0.1wt%-10wt%. Further preferably, the content of the reactive silicone resin in the modified PMMA resin is 0.5wt%-5wt%.

[0009] According to some preferred embodiments of the present invention, the molecular weight of the epoxy silicone oil is 5000-100000.

[0010] According to some embodiments of the present invention, the hydroxyl-containing olefinic monomer is selected from one or more of pentaerythritol triacrylate, dipentaerythritol pentaacrylate, pentaerythritol trimethacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, dimethacrylate glycerol, trimethylolpropane diallyl ether or trimethylolpropane monoacrylate. Further preferably, the hydroxyl-containing olefinic monomer is pentaerythritol triacrylate. Pentaerythritol triacrylate has three acrylic acid groups and one hydroxyl group, which is not only easier to be free radically polymerized with methyl methacrylate monomer, but also increases the crosslinking density, thereby improving the hardness, wear resistance and heat resistance of the product.

[0011] According to some embodiments of the present invention, the acid anhydride compound is selected from one or more of hexahydrophthalic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, methyl nadic anhydride, nadic anhydride, succinic anhydride or maleic anhydride.

[0012] According to some embodiments of the present invention, the method for preparing the reactive silicone resin comprises the following steps:

[0013] (1) An acid anhydride compound, a hydroxyl-containing olefin monomer, a polymerization inhibitor and a catalyst are mixed, heated to carry out an esterification reaction, and the next step is carried out when the acid value is reduced to the required value;

[0014] (2) Adding epoxy silicone oil and a catalyst to the reaction material of step (1), heating to carry out a ring-opening reaction, and the reaction is completed when the acid value is lower than 5 mgKOH / g to obtain the active silicone resin.

[0015] According to some embodiments of the present invention, in step (1), the heating temperature is 90-110°C.

[0016] According to some embodiments of the present invention, in step (2), the heating temperature is 90-110°C.

[0017] According to some embodiments of the present invention, the mass ratio of the anhydride compound, the hydroxyl-containing olefin monomer, the epoxy silicone oil, the polymerization inhibitor and the catalyst is (2-15): (2-25): (30-140): (0.01-0.1): (0.1-1). Further preferably, the mass ratio of the anhydride compound, the hydroxyl-containing olefin monomer, the epoxy silicone oil, the polymerization inhibitor and the catalyst is (2-10): (2-15): (60-110): (0.01-0.1): (0.1-1).

[0018] According to some embodiments of the present invention, the polymerization inhibitor is selected from one or more of p-hydroxyanisole, hydroquinone, tert-butylcatechol, tert-butylhydroquinone, benzoquinone, nitroxyl piperidinol, 2,5-di-tert-butylhydroquinone, 2,6-di-tert-butyl-p-cresol or phenothiazine. Different polymerization inhibitors affect the color of the product.

[0019] According to some embodiments of the present invention, the catalyst is selected from one or more of triphenylphosphine, p-toluenesulfonic acid, benzyltriethylammonium chloride, triethylamine, lithium hydroxide, tetrabutyl titanate, isopropyl titanate, potassium phosphate or calcium phosphate.

[0020] According to some embodiments of the present invention, the modified PMMA resin contains the following raw materials in parts by weight: 45-135 parts of methyl methacrylate, 0.1-10 parts of active silicone resin, 0-10 parts of functional monomer, 0-10 parts of plasticizer, and 0.01-1 parts of initiator.

[0021] According to some embodiments of the present invention, the plasticizer is tributyl citrate, and the initiator is azobisisobutyronitrile.

[0022] According to some embodiments of the present invention, the functional monomer is selected from one or more of styrene, methyl styrene, ethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, butyl acrylate, isooctyl acrylate, isobornyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, acrylonitrile, vinyl acetate, acrylamide, versatate, glycidyl methacrylate, divinylbenzene, lauryl methacrylate, ethyl acetoacetate methacrylate, octadecyl methacrylate, acrylic acid, methacrylic acid, bisphenol A epoxy acrylate, novolac epoxy acrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate and derivatives thereof.

[0023] The present invention further provides a PMMA product, comprising a PMMA substrate layer and a PMMA functional layer, wherein the PMMA functional layer is composited on the PMMA substrate layer, and the material of the PMMA functional layer is the modified PMMA resin.

[0024] The present invention also provides a method for preparing the PMMA product, comprising the following steps:

[0025] S1: preparing the PMMA substrate layer;

[0026] S2: mixing the raw materials for preparing the modified PMMA resin, heating and reacting, and obtaining a functional layer prepolymer resin when the viscosity and solid content of the reaction materials reach target values;

[0027] S3: placing the PMMA substrate layer in a mold, casting the functional layer prepolymer resin, and demoulding after curing to obtain the PMMA product.

[0028] According to some embodiments of the present invention, in step S2, the temperature of the heating reaction is 75-90°C.

[0029] According to some embodiments of the present invention, in step S2, the viscosity of the functional layer prepolymer resin is 150-200 cP, and the solid content is 15-20%.

[0030] According to a preferred embodiment of the present invention, there are at least the following beneficial effects:

[0031] 1. The modified PMMA resin of the present invention is mainly composed of active silicone resin and methyl methacrylate monomer. The methyl methacrylate monomer provides a molecular chain skeleton, and the active silicone resin provides hydrophobic functional branches anchored on the resin, so that the PMMA resin has stable and long-lasting hydrophobic properties. The price of epoxy silicone oil is low, with a unit price of several tens of yuan per kilogram, which greatly reduces the cost compared with fluorine-containing acrylic monomers.

[0032] 2. The present invention needs to use epoxy silicone oil with a large molecular weight. If the molecular weight is too small, the hydrophobicity will be weakened. If you want to obtain obvious hydrophobicity, you need to add a higher amount, which not only increases the cost, but also reduces the mechanical properties of the material such as hardness and strength. However, too large a molecular weight will also deteriorate the compatibility, making it difficult for the active silicone resin to disperse in the material, and the activity of the functional group will also be reduced, thereby affecting the chemical reaction rate. Experimental verification shows that the comprehensive effect of epoxy silicone oil with a molecular weight of 5000-500000 is better.

[0033] 3. Acid anhydride compounds convert the hydroxyl groups of olefin monomers into carboxyl groups, creating conditions for the subsequent reaction with epoxy silicone oil. In addition, due to the steric hindrance effect of macromolecular epoxy silicone oil, the active C=C double bond needs to be at a large spatial distance from the macromolecular siloxy chain of epoxy silicone oil to easily undergo free radical polymerization with methyl methacrylate monomer. Therefore, acid anhydride compounds are selected for bridging.

[0034] 4. The present invention obtains a PMMA product having anti-fouling and hydrophobic properties on one side and an easily bonded PMMA substrate on the other side by composite molding of a modified PMMA resin and an ordinary PMMA substrate layer, thereby achieving a stable easy-to-clean effect at a relatively low cost. The casting molding process ensures that the PMMA functional layer is tightly bonded to the PMMA substrate layer, and no peeling occurs during the secondary processing and molding of the product. The product can be subjected to secondary vacuum molding and is applicable to easy-to-clean bathtubs, star basins, wash basins and other products.

[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 This is a process flow chart of Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0039] The modified PMMA resin of the present invention is further described in detail below through specific preferred embodiments combined with comparative examples and effect test examples, but the present invention is not limited to the following embodiments.

[0040] Table 1 Recipes of reactive silicone resin, modified PMMA resin, and PMMA substrate

[0041]

[0042] The preparation process of Example 1 (refer to Figure 1 ):

[0043] 1. Preparation of active organosilicon resin: melt hexahydrophthalic anhydride into liquid at 60° C. in a water bath and add it into a reactor, then add p-hydroxyanisole, pentaerythritol triacrylate and triphenylphosphine, stir evenly and take a sample to measure the initial acid value, heat to 105° C. at a heating rate of 8° C. / h and keep the temperature for reaction for 120 min, take a sample, add an acetone aqueous solution to dissolve, test the acid value by potentiometric titration, when the acid value is reduced to half of the initial acid value, the first step of the reaction is completed, cool to below 60° C., add 6000 molecular weight epoxy silicone oil and triphenylphosphine, then heat to 105° C. at a heating rate of 8° C. / h and keep the temperature for reaction for 120 min, take a sample and add acetone to dissolve, then test the acid value by potentiometric titration, when the acid value is lower than 5 mgKOH / g, cool to below 40° C. to obtain an active organosilicon resin.

[0044] 2. Preparation of PMMA substrate layer: Methyl methacrylate, butyl acrylate, tributyl citrate and azobisisobutyronitrile are added to the prepolymerization kettle, stirring is turned on and the water pump is turned on to pass 80°C hot water into the jacket to heat the materials. After 30 minutes, samples are taken every 10 minutes to test the viscosity. When the viscosity is greater than 100cp, the viscosity and solid content are measured at the same time. When the viscosity is between 150-200cp and the solid content is between 15-20%, the temperature is lowered to 40°C to obtain a substrate prepolymer resin, which is cast into a glass mold to eliminate bubbles, cured in a 60°C water bath for 3 hours, then transferred to an oven at 120°C for curing for 2 hours, cooled to room temperature, and demolded to obtain a PMMA substrate layer.

[0045] 3. Preparation of easy-to-clean PMMA composite sheet (synthesis and molding of modified PMMA resin): Add methyl methacrylate, active silicone resin, butyl acrylate, tributyl citrate and azobisisobutyronitrile to the prepolymerization kettle, turn on the stirring and turn on the water pump to pass 80°C hot water into the jacket to heat the material. After 30 minutes, take samples every 10 minutes to test the viscosity. When the viscosity is greater than 100cp, measure the viscosity and solid content at the same time. When the viscosity is 150-200cp and the solid content is 15-20%, cool to 40°C to obtain a functional layer prepolymer resin, then clamp the PMMA substrate layer to the bottom of the glass mold, cast the functional layer prepolymer resin on it, and eliminate bubbles. Curing in a 60°C water bath for 3 hours, then transfer to an oven at 120°C for curing for 2 hours, cool to room temperature, and demold to obtain an easy-to-clean PMMA composite sheet.

[0046] The other embodiments and comparative examples refer to the above preparation process, and the feeding sequence can be adjusted according to the physicochemical properties of the raw materials.

[0047] Test example

[0048] The various properties of the PMMA composite sheets obtained in the examples and comparative examples were tested according to the following test methods. The results are shown in Table 2.

[0049] 1. Water contact angle: Contact angle measurement is carried out according to GB / T 30693-2014 standard.

[0050] 2. Friction resistance: Wrap a 10mm diameter, flat cylindrical friction head with 3 layers of non-woven fabric, then place a 1kg weight on it and rub it horizontally on the sample surface. The friction stroke is 65mm and the speed is 30 cycles / min. After 10,000 cycles of friction, observe whether the surface state of the sample is damaged and test the water contact angle.

[0051] 3. Water resistance: Immerse the sample in 80℃ pure water for 100 hours, observe whether there are defects such as blistering and gloss loss on the surface of the sample, and test the water contact angle.

[0052] 4. High temperature molding: Place the 1200x2400x4 (mm) sheet in a 190-200℃ oven for 6 minutes, then place it on a 1000x2000x500 (mm) rectangular vacuum forming mold for forming. De-mold it after cooling, tear off the protective film and observe whether there are defects such as gloss loss, pores, wrinkles, cracks, etc. on the surface.

[0053] 5. Oil-based pen stains are easy to scrub: Use the thick tip of a black zebra oil-based pen to draw a few stains. After drying for 30 minutes, wrap a 10mm diameter cylindrical friction head with 3 layers of non-woven fabric, moisten it with pure water, put a 1kg weight on it, rub it parallel to the stain 20 times, and observe whether the stain is wiped off.

[0054] 6. Barcol hardness: Use a Barcol hardness tester to measure the hardness of the plate surface.

[0055] 7. Scale adhesion and easy scrubbing: Put 100L of tap water in a 600x600x500 sink, then hang the sample to be tested vertically in the sink, half of it immersed in tap water and half exposed to the air, use a blower to blow air into the bottom of the sink, with a flow rate of 50L / min, so that the liquid surface is in a tumbling state for 30 minutes, then take out the sample and observe the scale adhesion. Leave it at room temperature for 24 hours to let the scale dry, wrap a cylindrical friction head with a diameter of 10mm with 3 layers of non-woven fabric, moisten it with pure water, put a 1kg weight on it, rub it on the scale in parallel for 20 times, and observe whether the scale is wiped off.

[0056] Table 2 Performance test results

[0057]

[0058] As can be seen from Table 2, the hydrophobic property of Comparative Example 1 is provided by perfluorodecyl acrylate, and even though its usage is much more than that of the embodiment, the hydrophobic effect is still not as good as that of the embodiment, and the price of perfluorodecyl acrylate is expensive, and the cost of raw materials is high. Comparative Example 2 uses epoxy silicone oil with a lower molecular weight, and even though the usage of epoxy silicone oil in the modified PMMA resin is equivalent to that of Example 3, the hydrophobic effect of Comparative Example 2 is still significantly reduced.

[0059] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A modified PMMA resin, characterized in that: The modified PMMA resin is obtained by copolymerizing methyl methacrylate and active silicone resin, and the active silicone resin is prepared by the following method: esterifying a hydroxyl-containing olefin monomer with an acid anhydride compound to obtain an intermediate with a single carboxyl group, and then performing a ring-opening reaction on the intermediate with a single carboxyl group and epoxy silicone oil to obtain the active silicone resin; wherein the molecular weight of the epoxy silicone oil is 5000-500000.

2. The modified PMMA resin according to claim 1, characterized in that The content of the active silicone resin in the modified PMMA resin is 0.1 wt %-10 wt %.

3. The modified PMMA resin according to claim 1, characterized in that The hydroxyl-containing olefin monomer is selected from one or more of pentaerythritol triacrylate, dipentaerythritol pentaacrylate, pentaerythritol trimethacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, glycerol dimethacrylate, trimethylolpropane diallyl ether or trimethylolpropane monoacrylate.

4. The modified PMMA resin according to claim 1, characterized in that The acid anhydride compound is selected from one or more of hexahydrophthalic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, methylnadic anhydride, nadic anhydride, succinic anhydride or maleic anhydride.

5. The modified PMMA resin according to claim 1, characterized in that The preparation method of the reactive silicone resin comprises the following steps: (1) An acid anhydride compound, a hydroxyl-containing olefin monomer, a polymerization inhibitor and a catalyst are mixed, heated to carry out an esterification reaction, and the next step is carried out when the acid value is reduced to the required value; (2) Adding epoxy silicone oil and a catalyst to the reaction material of step (1), heating to carry out a ring-opening reaction, and the reaction is completed when the acid value is lower than 10 mgKOH / g to obtain the active silicone resin.

6. The modified PMMA resin according to claim 5, characterized in that: The mass ratio of the acid anhydride compound, the hydroxyl-containing olefin monomer, the epoxy silicone oil, the polymerization inhibitor and the catalyst is (2-15): (2-25): (30-140): (0.01-0.1): (0.1-1).

7. The modified PMMA resin according to claim 1, characterized in that The modified PMMA resin comprises the following raw materials in parts by weight: 45-135 parts of methyl methacrylate, 0.1-10 parts of active silicone resin, 0-10 parts of functional monomer, 0-10 parts of plasticizer, and 0.01-1 parts of initiator.

8. The modified PMMA resin according to claim 7, characterized in that The functional monomer is selected from one or more of styrene, methyl styrene, ethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, butyl acrylate, isooctyl acrylate, isobornyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, acrylonitrile, vinyl acetate, acrylamide, versatate vinyl ester, glycidyl methacrylate, divinylbenzene, lauryl methacrylate, ethyl acetoacetate methacrylate, octadecyl methacrylate, acrylic acid, methacrylic acid, bisphenol A epoxy acrylate, novolac epoxy acrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate and derivatives thereof.

9. A PMMA product, characterized in that: It comprises a PMMA substrate layer and a PMMA functional layer, wherein the PMMA functional layer is composited on the PMMA substrate layer, and the material of the PMMA functional layer is the modified PMMA resin according to any one of claims 1 to 8.

10. The method for preparing a PMMA product according to claim 9, characterized in that: The following steps are involved: S1: preparing the PMMA substrate layer; S2: mixing the raw materials for preparing the modified PMMA resin, heating and reacting, and obtaining a functional layer prepolymer resin when the viscosity and solid content of the reaction materials reach target values; S3: placing the PMMA substrate layer in a mold, casting the functional layer prepolymer resin, and demoulding after curing to obtain the PMMA product.