Thermal activation type high-solid-content polyurethane emulsion and preparation method thereof

By using multiple chain extension reactions of polyester polyols, isocyanates and other components in heat-activated aqueous polyurethane adhesives, and the use of dihydroxysulfonate and ethylenediamine, combined with hydroxyethylpiperazine ethanesulfonic acid, the solution is solved The problems of low solid content and high activation temperature are achieved, and a polyurethane emulsion with high solid content and low activation temperature are simplified, and the process is reduced and energy consumption is reduced.

CN118994532APending Publication Date: 2024-11-22SHANGHAI LANOU CHEM IND TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078062.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing thermally activated aqueous polyurethane adhesives have low solid content and high activation temperature, which leads to large baking energy consumption and difficult process control.

Method used

Polyester polyols, isocyanates, chain extenders and catalysts are used to form a high-solid polyurethane emulsion through multiple chain extension reactions. Add isophorone diisocyanate and hexamethylene diisocyanate to reduce the activation temperature. Hydroxysulfonate and ethylenediamine improve the molecular weight and fluidity of the emulsion, and the addition of hydroxyethylpiperazine ethanesulfonic acid improves wetting and mechanical properties.

Benefits of technology

The solid content is greater than 50%, the activation temperature is reduced to less than 61°C, the process flow is simplified, the baking energy consumption is reduced, and the bonding strength and fluidity are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982922680000041
    Figure BDA0004982922680000041
  • Figure BDA0004982922680000051
    Figure BDA0004982922680000051
  • Figure BDA0004982922680000061
    Figure BDA0004982922680000061
Patent Text Reader

Abstract

The invention relates to the technical field of organic high-molecular polymers, and particularly discloses a thermal activation type high-solid-content polyurethane emulsion and a preparation method thereof. The thermal activation type high-solid-content polyurethane emulsion is prepared from the following components in parts by weight: 80 to 85 parts of polyester polyol; 1-3 parts of polyether; 14 to 16 parts of isocyanate; 4-6 parts of a chain extender; 0.1 to 0.2 part of a catalyst; 300 parts of an organic solvent; 300 parts of water; 1.5 to 2 parts of hydroxyethyl piperazine ethanesulfonic acid; the isocyanate is prepared from isophorone diisocyanate and hexamethylene diisocyanate; the chain extender is prepared from 1, 4-butanediol, dihydroxy sulfonate and ethidene diamine. The thermal activation type high-solid-content polyurethane emulsion can be used for preparing an adhesive, has the advantages of being high in solid content and low in activation temperature, and is good in fluidity, high in adhesive strength and excellent in mechanical property after emulsion film forming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of organic high molecular polymers, and more specifically, to a heat-activated high-solid polyurethane emulsion and a preparation method thereof. Background Art Heat-activated water-based polyurethane adhesive is a new type of ionic polyurethane adhesive. It is a liquid adhesive that makes the adhesive film sticky by heating to complete bonding. Its principle is: after the water-based adhesive is evenly dispersed in the bonding object, the crystal chain segments of the adhesive film melt at the heat activation temperature, and the adhesive film restores fluidity and adhesion to form an adhesive layer. After drying and cooling, it becomes a thin film covering the surface of the substrate to complete the bonding.

[0003] The main raw material of the adhesive, water-based polyurethane resin, is an environmentally friendly polymer material with water as the dispersion medium. It has the advantages of being non-flammable, low odor, non-polluting, energy-saving, and easy to operate and process. It generally uses aminosulfonic acid or hydroxycarboxylic acid as a hydrophilic monomer. Due to the high reactivity of amino groups with isocyanates, it can generally only be added slowly in the later stage, and the process control is difficult. There is no process difficulty in the use of hydroxycarboxylic acid, but due to the weak acidity and low salt-forming property of carboxylic acid, the solid content of water-based polyurethane is low, only 30-40%, and the activation temperature is also high, resulting in the need for more baking energy. Summary of the invention

[0004] In order to increase the solid content of an aqueous polyurethane emulsion and reduce its activation temperature, the present application provides a heat-activated high-solid polyurethane emulsion and a preparation method thereof.

[0005] In the first aspect, the present application provides a heat-activated high-solid polyurethane emulsion, which adopts the following technical solution: A heat-activated high-solid polyurethane emulsion comprises the following components in parts by weight: 80-85 parts of polyester polyol; Polyether 1-3 parts; Isocyanate 14-16 parts; 4-6 parts of chain extender; Catalyst 0.1-0.2 parts; 300 parts of organic solvent; 300 parts water; The isocyanate includes isophorone diisocyanate and hexamethylene diisocyanate; The chain extender includes 1,4-butanediol, dihydroxy sulfonate and ethylenediamine.

[0006] By adopting the above technical scheme: the emulsion uses polyester polyol and isocyanate as raw materials, 1,4-butanediol, dihydroxysulfonate and ethylenediamine as chain extenders, and after multiple chain extensions, a polyester-type water-based polyurethane emulsion is obtained, and its peel strength is greater than that of a polyether-type polyurethane emulsion. Among them, IPDI is used as isocyanate to increase the bonding strength of the emulsion, HDI is added to reduce the activation temperature, dihydroxysulfonate is used as the hydrophilic monomer, and no later addition is required, polydiethanol hydrophilic polyether is used to improve the emulsification performance, improve the fluidity and wettability of the emulsion, and ethylenediamine is used to increase the molecular weight of the emulsion, thereby obtaining a low activation temperature and high solid content polyurethane emulsion, which can be better used in adhesives.

[0007] According to the test, the thermal activation temperature of the prepared polyurethane emulsion is within 61°C and the solid content is greater than 50%.

[0008] Optionally, the weight ratio of isophorone diisocyanate to hexamethylene diisocyanate is (1.8-2.2):1.

[0009] By adopting the above technical solution: IPDI increases the bonding strength of the emulsion, and HDI is added to reduce the activation temperature. When the amounts of the two are within the above range, the comprehensive performance of the prepared polyurethane emulsion is better.

[0010] Optionally, the polyester polyol is a polyester diol having a molecular weight of 2000-3000 or a combination thereof.

[0011] By adopting the above technical solution: using polyester diols with a molecular weight within the above range, the crystallinity and bonding properties of the polyol are balanced.

[0012] Optionally, the polyester polyol is a mixture of polybutylene adipate diol with a molecular weight of 2000 and polyhexylene adipate diol with a molecular weight of 3000 in a weight ratio of (3-3.25):1.

[0013] By adopting the above technical solution: compounding polybutylene adipate diol with a molecular weight of 2000 and polyhexylene adipate diol with a molecular weight of 3000, the prepared polyurethane emulsion has better crystallization performance and adhesion.

[0014] Optionally, the polyether is polyethylene glycol with a molecular weight of 1000.

[0015] Optionally, the catalyst is dibutyltin dilaurate.

[0016] Optionally, the organic solvent is acetone.

[0017] Optionally, the dihydroxy sulfonate is sodium 1,2-dihydroxy-3-propanesulfonate.

[0018] Optionally, the polyurethane emulsion further comprises the following components in parts by weight: 1.5-2 parts of hydroxyethylpiperazineethanesulfonic acid.

[0019] By adopting the above technical solution: the addition of polyether will improve the fluidity and wettability of the emulsion by increasing the droplet size. As the amount of polyether added increases, the tensile strength and elongation at break of the formed film will first increase and then decrease, which may be because the introduction of polyether destroys the orderly arrangement of the long-chain molecules of the soft segment. Therefore, further improvement is made by adding hydroxyethylpiperazineethane sulfonic acid, and the wettability and fluidity of the prepared emulsion are better, and the tensile strength after film formation is increased.

[0020] The reasons may be: Hydroxyethylpiperazine ethane sulfonic acid is hydrolyzed in aqueous solution to form hydroxyethylpiperazine and ethane sulfonic acid. Hydroxyethylpiperazine promotes the long-range orderly arrangement between the emulsion molecules, thereby improving the mechanical properties of the formed film. Ethane sulfonic acid is acidic and reduces the pH of the emulsion. The electric repulsion between the emulsion droplets due to the Zata potential is reduced. Subsequently, under the high temperature conditions of the emulsion reaction, the emulsion droplets with lower Zata potential will polymerize and increase the particle size. Therefore, it has a synergistic effect on the polyether to increase the emulsion droplet size and jointly reduce the apparent viscosity of the emulsion to improve the wettability and fluidity of the emulsion.

[0021] In a second aspect, the present application provides a method for preparing a heat-activated high-solid polyurethane emulsion, using the following technical solution: A method for preparing a heat-activated high-solid polyurethane emulsion comprises the following steps: S1, blending polyester polyol, polyether, 1,4-butanediol and dihydroxy sulfonate, adding isophorone diisocyanate, hexamethylene diisocyanate and a catalyst, heating to react, adding an organic solvent and mixing to obtain a prepolymer; S3, cooling the prepolymer and mixing it with water, then adding ethylenediamine, reacting, and evaporating the organic solvent to obtain the product.

[0022] By adopting the above technical scheme: polyester polyol, hydrophilic chain extender dihydroxy sulfonate, small molecule chain extender 1,4-butanediol, isophorone diisocyanate and hexamethylene diisocyanate are reacted to obtain a prepolymer, and then water is added for emulsification, and ethylenediamine is added for a second chain extension to increase the molecular weight, thereby obtaining a waterborne polyurethane emulsion. The overall steps are relatively few, the process is simple and efficient, and the obtained polyurethane emulsion has the advantages of high solid content and low activation temperature, does not require much baking energy, and is beneficial to energy saving and environmental protection.

[0023] In summary, this application has the following beneficial effects: 1. The present application uses isophorone diisocyanate and hexamethylene diisocyanate as raw materials. Hexamethylene diisocyanate reduces the activation temperature. The first chain extension reaction is carried out through 1,4-butanediol and dihydroxysulfonate. The process is easy to control. The second chain extension reaction is carried out through ethylenediamine to increase the molecular weight of the emulsion, thereby obtaining a polyurethane emulsion with high solid content and low activation temperature. 2. In the present application, it is preferred to control the ratio of isophorone diisocyanate and hexamethylene diisocyanate, control the molecular weight of polyester polyol, and balance the comprehensive properties of polyurethane emulsion such as crystallinity, adhesion, activation temperature, etc.; 3. The polyurethane emulsion of the present application is also specially added with hydroxyethylpiperazine ethane sulfonic acid, which is hydrolyzed into hydroxyethylpiperazine and ethane sulfonic acid, and together with the polyether, improves the wettability and fluidity of the emulsion, and enhances the mechanical properties of the film formed by the emulsion. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] The sources of the components are as follows. Except for the following special instructions, the components are commercially available: PBA2000 (polybutylene adipate diol) was purchased from Zhejiang Huafeng New Materials Co., Ltd., model PE-3020; PHA3000 (poly(hexanediol adipate) diol) was purchased from Zhejiang Huafeng New Materials Co., Ltd., model PE-9937; IPDI (isophorone diisocyanate), brand is Covestro of Germany; HDI (hexamethylene diisocyanate), the brand is Covestro of Germany.

[0026] Examples 1-3, Comparative Examples 1-2 A heat-activated high-solid polyurethane emulsion, the components and their corresponding weights are shown in Table 1, and is prepared by the following steps: S1. Raise the temperature to 60°C, add polyester polyol (PBA2000, PHA3000), polyether (PEG-1000) 1,4-butanediol, and sodium 1,2-dihydroxy-3-propanesulfonate, stir and mix at a speed of 300 rpm for 30 min, dropwise add isocyanate (isophorone diisocyanate and hexamethylene diisocyanate), the reaction is exothermic and the temperature rises naturally during the dropwise addition, add catalyst dibutyltin dilaurate after the temperature stabilizes, then raise the temperature to 85°C for reaction for 1 h, add acetone, stir and mix at a speed of 300 rpm for 30 min, and obtain a prepolymer; S3. Cool the prepolymer to 40°C, stir and mix at a speed of 800 rpm for 10 minutes, first add water accounting for 10% of the total water within 10 minutes, stir and mix, then add the remaining water at once, continue to stir and mix for 10 minutes, then add ethylenediamine, keep the reaction warm for 0.5 hours, distill off acetone at -0.05 MPa to obtain a polyurethane emulsion.

[0027] It should be noted that in the preparation step S1 of the polyurethane emulsion of the present application, the heating temperature can be selected within the range of 80-90°C, and the cooling temperature in step S2 can be selected within the range of 35-45°C. The above selection does not have a significant impact on the performance test results. In the embodiments of the present application, only one of the temperatures is briefly introduced as an example.

[0028] Table 1 Components and their weights (g) in Examples 1-3 and Comparative Examples 1-2 Comparative Example 3 A polyurethane emulsion, which is different from Example 2 in that an equal amount of isophorone diisocyanate is used instead of hexamethylene diisocyanate.

[0029] Comparative Example 4 A polyurethane emulsion, which differs from Example 2 in that ethylenediamine is not added for secondary chain extension, and the specific preparation method of the emulsion is: S1. Raise the temperature to 60°C, add polyester polyol (PBA2000, PHA3000), polyether (PEG-1000) 1,4-butanediol, and sodium 1,2-dihydroxy-3-propanesulfonate, stir and mix at a speed of 300 rpm for 30 min, dropwise add isocyanate (isophorone diisocyanate and hexamethylene diisocyanate), the reaction is exothermic and the temperature rises naturally during the dropwise addition, add catalyst dibutyltin dilaurate after the temperature stabilizes, then raise the temperature to 85°C for reaction for 1 h, add acetone, stir and mix at a speed of 300 rpm to obtain a prepolymer; S3. Cool the prepolymer to 40°C, stir and mix at a speed of 800 rpm for 10 minutes, add 10% of water in 10 minutes, stir and mix, add the remaining water at once, continue stirring and mixing for 30 minutes, and distill off acetone at -0.05 MPa to obtain.

[0030] Embodiment 4-6 A heat-activated high-solid polyurethane emulsion, the components and their corresponding weights are shown in Table 2, and is prepared by the following steps: S1. Raise the temperature to 60°C, add polyester polyol (PBA2000, PHA3000), polyether (PEG-1000) 1,4-butanediol, and sodium 1,2-dihydroxy-3-propanesulfonate, stir and mix at a speed of 300 rpm, and dropwise add isocyanate (isophorone diisocyanate and hexamethylene diisocyanate). During the dropwise addition, the reaction is exothermic and the temperature rises naturally. After the temperature stabilizes, add catalysts such as dibutyltin dilaurate and hydroxyethylpiperazineethane sulfonic acid, and then raise the temperature to 85°C for reaction for 1 hour. Add acetone, stir and mix at a speed of 300 rpm to obtain a prepolymer; S3. Cool the prepolymer to 40°C, stir and mix at a speed of 800 rpm, first add 10% of water in 10 minutes, stir and mix, then add the remaining water at once, continue to stir and mix, then add ethylenediamine, keep the temperature for reaction for 0.5 hours, and distill off acetone at -0.05 MPa to obtain a polyurethane emulsion.

[0031] Table 1 Components and their weights in Examples 4-6 (g) Performance Testing The following performance tests were performed on the polyurethane emulsions prepared in the examples and comparative examples, and the test results are recorded in Table 3.

[0032] Detection Methods Preparation of the sample: Polyurethane emulsion at 70g / m 2 Apply the amount of glue on the surface of PVC leather, put it into a circulating air drying oven at 140℃ and dry it for 3 minutes, take it out and place it at room temperature for 24 hours.

[0033] 1. Thermal activation temperature: Place a 1cm×2cm sample on a PVC sheet, heat treat it in an oven for 20 minutes, and gently press the PVC sheet. When the sample melts and becomes sticky and has a certain adhesive force, the heat treatment temperature is considered to be the thermal activation temperature of the polyurethane emulsion.

[0034] 2. Tensile strength: The tensile strength of the specimens was tested according to GB1040-79, and the tensile rate during the test was 50 mm / min.

[0035] 3. Peel strength: The emulsion was tested according to GB / T 2791-1995.

[0036] 4. Apparent viscosity: The emulsion is measured at 25°C using a NDJ-79 rotary viscometer. The smaller the apparent viscosity, the better the fluidity of the emulsion.

[0037] Table 3 Performance test results Referring to Table 3, Examples 1-3 use PBA2000, PHA3000, isophorone diisocyanate and hexamethylene diisocyanate as raw materials, extend the chain through 1,4-butanediol, dihydroxy sulfonate and ethylenediamine, and control the dosage range of each component, so the obtained polyurethane emulsion has the characteristics of high solid content and low activation temperature; while the dosage of the components in Comparative Examples 1-2 is different, hexamethylene diisocyanate is not used in Comparative Example 3, and ethylenediamine is not used for secondary chain extension in Comparative Example 4, and the performance of the prepared polyurethane emulsion is reduced.

[0038] The difference between Example 4-6 and Example 2 is that hydroxyethylpiperazineethanesulfonic acid is also added during the preparation of the polyurethane emulsion, and the tensile and peel strengths of the prepared emulsions are improved, and the apparent viscosity is significantly reduced, indicating that hydroxyethylpiperazineethanesulfonic acid can enhance the adhesion and fluidity of the polyurethane emulsion, and enhance the mechanical properties of the formed film.

[0039] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A heat-activated high-solid polyurethane emulsion, characterized in that: The composition comprises the following components in parts by weight: 80-85 parts of polyester polyol; Polyether 1-3 parts; Isocyanate 14-16 parts; 4-6 parts of chain extender; Catalyst 0.1-0.2 parts; 300 parts of organic solvent; 300 parts water; The isocyanate includes isophorone diisocyanate and hexamethylene diisocyanate; The chain extender includes 1,4-butanediol, dihydroxy sulfonate and ethylenediamine.

2. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The weight ratio of isophorone diisocyanate to hexamethylene diisocyanate is (1.8-2.2):

1.

3. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The polyester polyol is a polyester diol with a molecular weight of 2000-3000 or a combination thereof.

4. A heat-activated high-solid polyurethane emulsion according to claim 3, characterized in that: The polyester polyol is a mixture of polybutylene adipate diol with a molecular weight of 2000 and polyhexylene adipate diol with a molecular weight of 3000 in a weight ratio of (3-3.25):

1.

5. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The polyether is polyethylene glycol with a molecular weight of 1000.

6. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate.

7. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The organic solvent is acetone.

8. A heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The dihydroxy sulfonate is sodium 1,2-dihydroxy-3-propanesulfonate.

9. The heat-activated high-solid polyurethane emulsion according to claim 1, characterized in that: The polyurethane emulsion further comprises the following components in parts by weight: 1.5-2 parts of hydroxyethylpiperazineethane sulfonic acid.

10. A method for preparing the heat-activated high-solid polyurethane emulsion according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, blending polyester polyol, polyether, 1,4-butanediol and dihydroxy sulfonate, adding isophorone diisocyanate, hexamethylene diisocyanate and a catalyst, heating to react, adding an organic solvent and mixing to obtain a prepolymer; S3, cooling the prepolymer and mixing it with water, then adding ethylenediamine, reacting, and evaporating the organic solvent to obtain the product.