2, 5-furandicarboxylic acid-based copolyester and synthesis method thereof

Through the copolymerization of 2,5-furandicarboxylic acid FDCA with dibasic acid and diol, combined with germanium titanium catalyst and high temperature and high vacuum polycondensation, the problems of poor barrier properties and complex preparation of bio-based copolyester are solved, and high Properties and low cost biobased copolyester material preparation.

CN118994547APending Publication Date: 2024-11-22HEFEI LEAF BIOTECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411241605.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing bio-based copolyesters have poor gas barrier properties, complex preparation methods, long reaction times and high cost.

Method used

Copolymerization of 2,5-furandicarboxylic acid FDCA with specific structure dibasic acid and diol is prepared by esterification and polycondensation reaction, using germanium-titanium composite catalyst and polycondensation under high temperature and high vacuum conditions, optimized Reaction conditions are used to reduce the end carboxylic content and increase the molecular weight.

Benefits of technology

Bio-based copolyesters with good mechanical properties and gas barrier properties were obtained, reducing reaction costs, simplifying the preparation process, and improving the polymerization rate and product viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994547A_ABST
    Figure CN118994547A_ABST
Patent Text Reader

Abstract

The invention discloses 2, 5-furandicarboxylic acid-based copolyester and a synthesis method thereof, and relates to the field of synthesis of bio-based polyester. According to the invention, 2, 5-furandicarboxylic acid, binary acid and dihydric alcohol are used as raw materials, and under the action of additives such as a catalyst, an antioxidant and a stabilizer, esterification and condensation polymerization are carried out to prepare the 2, 5-furandicarboxylic acid copolyester. Compared with the traditional synthesis of polyethylene glycol terephthalate, no catalyst needs to be added in the esterification step, and the reaction cost is further reduced by introducing 2, 5-furandicarboxylic acid into the copolyester structure. The synthesized copolyester keeps good mechanical properties and also has excellent gas barrier property, and can be widely applied to the fields of fibers, films, packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bio-based copolyesters, and specifically relates to a 2,5-furandicarboxylic acid-based copolyester and a synthesis method thereof. Background Art

[0002] 5-Hydroxymethylfurfural (5-HMF), as the only platform-based compound with an aromatic ring, has high chemical reactivity and can be converted into high-value-added downstream derivatives such as 2,5-furandicarboxylic acid (FDCA), tetrahydrofuran dimethanol (THFDM), and 2,5-furan dimethanol (BAMF). These derivatives can be used as raw materials to make various products and are widely used in the fields of polyester, fiber, aramid, adhesives, plastics, etc. For example, FDCA can be used with ethylene glycol to prepare polyethylene 2,5-furandicarboxylate (PEF) through polymerization. PEF, as the most promising alternative to polyethylene terephthalate (PET), is a bio-based functional polyester material with superior performance. It can be used in scenarios with high requirements for barrier properties and heat resistance, such as packaging, medical consumables, and other fields.

[0003] Compared with PET, although PEF has higher gas barrier properties and excellent thermomechanical properties, it has problems such as poor toughness and ductility, slow crystallization rate, etc. In order to improve the comprehensive performance of PEF, performance complementarity can be achieved through copolymerization, blending, nano-composite and other methods. Patent CN115926396A studies the barrier properties enhanced by blends of PET and PEF. Adding a relatively small amount of PEF during the preparation of PET bottles can produce bottles with the desired barrier properties. Based on the success of FDCA binary polymerization, researchers began to explore the ternary polymerization of FDCA. Patent CN112760740B provides a bio-based FDCA-based copolyester fiber and its preparation method and application. FDCA-based copolyester is prepared by reacting a mixed system of FDCA, terephthalic acid (PTA), ethylene glycol, glycol ether, esterification catalyst, polycondensation catalyst, stabilizer and antioxidant. Patent CN102432847B provides a 2,5-furandicarboxylic acid-terephthalic acid-aliphatic diol ester and a preparation method thereof. FDCA, PTA and aliphatic diol ester first undergo esterification reaction under the action of tin or titanium catalysts to generate a first intermediate product, and then undergo polycondensation reaction under the action of phosphorus compounds to obtain 2,5-furandicarboxylic acid-terephthalic acid-aliphatic diol ester. The copolyester has good properties comparable to PET, and can therefore be used to prepare films and engineering plastics. In addition, since 2,5-thiophenedicarboxylic acid (TDCA) has a similar structure to FDCA and PTA, it can also be used in the field of polyester synthesis. Patent CN109553765A discloses a 2,5-thiophenedicarboxylic acid-based copolyester and a preparation method thereof. The 1,4-cyclohexanedimethanol group introduced into the polyester is bonded to furandicarboxylic acid to increase the interaction between molecules, thereby increasing the glass transition temperature of the polyester material. Patent CN110734542A discloses a thiophenedicarboxylic acid-based copolyester and its preparation method and application. This type of copolyester has low melt viscosity, high light transmittance and molecular weight, and also has high gas barrier properties, and can be used in packaging materials, fibers, films and other fields.

[0004] Based on this, this patent provides a 2,5-furandicarboxylic acid-based copolyester and a synthesis method thereof, using dibasic acid, FDCA and diol as raw materials, and preparing FDCA-based copolyester through esterification and polycondensation reaction under the action of catalyst, antioxidant and stabilizer. The catalyst described in the present invention is a composite catalyst. Unlike the synthesis of traditional PET polyester, no catalyst is required in the esterification step, thereby reducing the reaction cost. In addition, FDCA copolyester has a lower terminal carboxyl content, and while maintaining good mechanical properties, it also has relatively good gas barrier properties. Summary of the invention

[0005] One of the purposes of the present invention is to provide a 2,5-furandicarboxylic acid-based copolyester to solve the problem that the existing bio-based copolyester has poor gas barrier properties;

[0006] The second object of the present invention is to provide a method for synthesizing 2,5-furandicarboxylic acid-based copolyester to solve the problems of complex process, long reaction time, high cost and the like in the existing preparation methods of bio-based polyester.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] In the first aspect, a 2,5-furandicarboxylic acid-based copolyester is a compound of formula I:

[0009]

[0010] Where Ar is R is one of -H, alkyl, and aryl, wherein R cannot be -H at the same time, the alkyl is preferably methyl, and the aryl is preferably phenyl;

[0011] n is an integer between 2 and 10, preferably 2, 3 or 4;

[0012] x and y are average polymerization degrees, x=1-150; y=1-150.

[0013] In a second aspect, a method for synthesizing 2,5-furandicarboxylic acid-based copolyester comprises the following steps:

[0014] 2,5-furandicarboxylic acid (FDCA) is mixed with a dibasic acid to obtain a mixed acid, and a diol is added to the mixed acid for esterification reaction to generate a first intermediate and water; a germanium-titanium composite catalyst, an antioxidant and a phosphorus stabilizer are added to the first intermediate for melt polycondensation reaction to obtain a 2,5-furandicarboxylic acid-based copolyester.

[0015] Further, the dibasic acid is R is one of -H, alkyl, and aryl, wherein R cannot be -H at the same time, the alkyl is preferably methyl, and the aryl is preferably phenyl;

[0016] Furthermore, the diol includes but is not limited to ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, and 1,8-octanediol; preferably, the diol is any one of ethylene glycol, 1,3-propylene glycol, or 1,4-butanediol.

[0017] Furthermore, the germanium-titanium composite catalyst is compounded by a germanium-based catalyst and a titanium-based catalyst in a mass ratio of 20-50:1; preferably, the mass ratio of the germanium-based catalyst to the titanium-based catalyst is 30:1.

[0018] Furthermore, the germanium-based catalyst includes one or more of germanium oxide, sodium germanate, and tetrabutoxygermanium; the titanium-based catalyst includes one or more of titanates (tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, etc.), titanium glycol, titanium acetylacetonate, 2-ethylhexyl titanium, potassium hexafluorotitanium, and titanium dioxide.

[0019] Furthermore, the antioxidants include but are not limited to antioxidant 1010, antioxidant 1178, antioxidant 1076, antioxidant 618, antioxidant 425, antioxidant 330, antioxidant 626, and antioxidant 168.

[0020] Furthermore, the stabilizer is a phosphorus-based stabilizer, including but not limited to triphenyl phosphate, triphenyl phosphite, ethyl phosphate, phosphoric acid, trimethyl phosphate, trimethyl phosphite, and polyphosphoric acid.

[0021] Furthermore, the molar ratio of the dibasic acid to FDCA is 0.1-1:1.

[0022] Furthermore, the molar ratio of the mixed acid to the diol is 1:1.05-2.0.

[0023] As a further solution of the present invention, the amount of the germanium-titanium composite catalyst is 0.01%-1% of the total mass of FDCA, dibasic acid and diol.

[0024] As a further solution of the present invention, the amount of the antioxidant is 0.01%-0.2% of the total mass of FDCA, dibasic acid and diol.

[0025] As a further solution of the present invention, the amount of the phosphorus stabilizer used is 0.01%-0.2% of the total mass of FDCA, dibasic acid and diol.

[0026] As a further solution of the present invention, the temperature of the esterification reaction is 185-235° C., the reaction time is 70-200 min, and the reaction pressure is 0.1-0.25 MPa.

[0027] As a further solution of the present invention, the temperature of the polycondensation reaction is 230-265° C., the reaction time is 120-360 min, and the reaction pressure is 1-100 Pa.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. The present invention provides a 2,5-furandicarboxylic acid-based copolyester, which is synthesized by copolymerization of FDCA, a dibasic acid of a specific structure and a diol, and has a low terminal carboxyl content, a high molecular weight and viscosity, thereby giving the bio-based copolyester material good mechanical properties and barrier properties. Among them, after the dicarboxylic acid containing a benzene ring is polymerized into a molecular chain, it has strong rigidity, and the dicarboxylic acid containing a five-membered heterocyclic ring has a similar structure to the benzene ring. After polymerizing into a high molecular chain, it can form a linear macromolecular structure. While the five-membered heterocyclic ring brings specific functions, the integrity of the chain is guaranteed. The methyl substituent can act as a "snap" between molecular chains to limit the movement of macromolecules, forming a π-π stacking and tight stacking, so that the material has good barrier properties.

[0030] 2. In the synthesis method of 2,5-furandicarboxylic acid-based copolyester, since the terminal carboxyl content is an important indicator of polyester and has a great influence on the physical properties and processability of polyester products, the present invention optimizes the reaction conditions to make the prepared bio-based copolyester have a lower terminal carboxyl content, higher molecular weight and viscosity. The germanium-titanium composite catalyst is added only in the polycondensation step to ensure that the catalytic activity of the thermal degradation side reaction is small while also improving the catalytic activity and reducing the reaction cost. In addition, the polycondensation reaction is carried out under high temperature and high vacuum conditions, which can increase the polymerization reaction rate and polymerization degree, thereby further increasing the viscosity of the product.

[0031] 3. The present invention uses the biomass platform molecule FDCA as raw material, which is derived from bio-based monomers and has the advantages of being green, environmentally friendly, and renewable. At the same time, the preparation method of FDCA-based copolyester also has the advantages of mild reaction conditions, environmental friendliness, and high yield, and can be widely used in fields such as plastics, films, and fibers that require high gas barrier properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be further described below in conjunction with the accompanying drawings;

[0033] Figure 1 It is a schematic diagram of the preparation process of the FDCA-based copolyester of the present invention;

[0034] Figure 2 is the chemical structural formula of the FDCA-based copolyester of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The relevant characterization test analysis methods in the following embodiments are as follows:

[0037] Molecular weight test: The molecular weight of copolyesters was determined by gel permeation chromatography (GPC);

[0038] Viscosity test: The viscosity test method refers to GB / T 14190-2017, using an Ubbelohde viscometer (manufacturer: Hangzhou Zhongwang Technology Co., Ltd.) at a constant temperature of 25°C. The solvent is a phenol / tetrachloroethane mixed solution with a concentration of 0.5 g / L and a mass ratio of 3 / 2.

[0039] Hue test: The slice hue test refers to the drying method in GB / T 14190-2017. After the sample is dried, the sample chromaticity is tested with a colorimeter (model DS-700D, manufacturer: Shenzhen Huaruichang Technology Co., Ltd.), and the average value of the calculated results of the two cups of samples is taken as the b value and L value.

[0040] L value is a representation of whiteness. The larger the L value, the greater the whiteness and the higher the brightness.

[0041] The b value is a representation of yellow color, and a large b value indicates a large yellow color;

[0042] The a value is not counted and is not considered as an indicator.

[0043] Diethylene glycol content test: The diethylene glycol content test refers to the methanol transesterification method in GB / T 14190-2017. The sample undergoes an ester exchange reaction under high temperature and the presence of methanol, and diethylene glycol is released. Then the diethylene glycol content in the filtrate is detected by gas chromatography.

[0044] Ethylene glycol (EG) undergoes its own synthesis reaction under high temperature conditions to produce diethylene glycol (DEG), which enters the polyester chain in the form of an ether bond. The existence of the ether bond affects the structure and molecular configuration of the polymer, causing the melting point and glass transition temperature to drop, the heat resistance and light resistance to deteriorate, and the hydrolysis stability to be damaged.

[0045] Terminal carboxyl content test: The terminal carboxyl content test refers to the volumetric titration method in GB / T 14190-2017.

[0046] The terminal carboxyl groups are mainly produced in two stages: esterification reaction and polycondensation reaction. The content of terminal carboxyl groups will affect the color value and stability of polyester chips, and thus affect the quality of the chips.

[0047] Gas permeability test

[0048] The TDCA-based copolyester was prepared into film samples by melt hot pressing, and the oxygen and carbon dioxide permeability coefficients P at 35°C were tested using a VAC-V1 differential pressure gas permeometer. O2 , P CO2, refer to the national standard GB / T 1038-2022; use WB-31 water vapor permeability tester to test the water vapor permeability coefficient P at 35°C H2O , refer to national standard GB / T 1037-2021.

[0049] Mechanical testing

[0050] Tensile test: Use a micro twin-screw extruder and a micro-injection instrument to inject the sample to be tested into a dumbbell-shaped specimen strip, and test it according to ASTMD 412a rules. The number of test specimen strips is generally 3-5, and the average value of the obtained data is taken as the final result.

[0051] For the schematic diagram of the synthesis process of 2,5-furandicarboxylic acid-based copolyester in the following examples, please refer to Figure 1 , chemical structure formula see Figure 2 .

[0052] Example 1

[0053] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester comprises the following steps:

[0054] 0.9 mol FDCA (140.5 g) and 0.1 mol 3,4-dimethylfuran-2,5-dicarboxylic acid (18.4 g) were added to a slurry tank to obtain a mixed acid, and 1.6 mol ethylene glycol (EG 99.3 g) was simultaneously conveyed to the mixed acid through a pipeline. The mixed acid and ethylene glycol were fully mixed in the slurry tank and then entered into an esterification tank. The reaction was stopped at a pressure of 0.25 MPa and a temperature of 210° C. for 2 h to obtain a first intermediate and water, and the water was discharged;

[0055] The first intermediate is transported to the polycondensation kettle through a pipeline, a bypass is set on the pipeline from the esterification tank to the polycondensation kettle, 1291 mg of a germanium-titanium composite catalyst prepared by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 (the amount of the germanium-titanium composite catalyst is 0.5% of the total mass of the mixed acid and ethylene glycol), 258.2 mg of triphenyl phosphate (the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol) and 258.2 mg of antioxidant 1010 (the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol) are added, and the mixture is put into the polycondensation kettle for melt polycondensation reaction. The reaction is stopped after reacting for 4 hours under the conditions of a pressure of 50 Pa and a temperature of 245° C. to obtain a product, poly-2,5-furandicarboxylic acid-3,4-dimethylfuran-2,5-dicarboxylic acid ethylene glycol copolyester, the structural formula of which is shown in Formula II:

[0056]

[0057] After testing: the viscosity is 0.77 dL / g, the slice b value is 5.3, the slice L value is 80, the diethylene glycol content is 1.25%, the terminal carboxyl content is 25.5 mol / t, and the molecular weight is 37482.

[0058] Example 2

[0059] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that the molar ratio of a mixed acid to ethylene glycol is 1:1.2, i.e., the amount of ethylene glycol is replaced by 1.2 mol, 74.5 g; on the basis of ensuring that the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1167 mg, the amount of triphenyl phosphate is 233.4 mg, and the amount of antioxidant 1010 is 233.4 mg; and the remaining steps and parameters remain the same.

[0060] After testing: the viscosity is 0.60 dL / g, the slice b value is 6.5, the slice L value is 74, the diethylene glycol content is 1.40%, the terminal carboxyl content is 35.5 mol / t, and the molecular weight is 27683.

[0061] Example 3

[0062] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that the molar ratio of a mixed acid to ethylene glycol is 1:1.4, i.e., the amount of ethylene glycol is replaced by 1.4 mol, 86.9 g; on the basis of ensuring that the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1229 mg, the amount of triphenyl phosphate is 245.8 mg, and the amount of antioxidant 1010 is 245.8 mg; and the remaining steps and parameters remain the same.

[0063] After testing: the viscosity is 0.65dL / g, the slice b value is 5.7, the slice L value is 78, the diethylene glycol content is 1.36%, the terminal carboxyl content is 30.3mol / t, and the molecular weight is 31658.

[0064] Example 4

[0065] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that the molar ratio of a mixed acid to ethylene glycol is 1:2, that is, the amount of ethylene glycol is replaced by 2 mol, 124 g; on the basis of ensuring that the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1414.5 mg, the amount of triphenyl phosphate is 282.9 mg, and the amount of antioxidant 1010 is 282.9 mg; and the remaining steps and parameters remain the same.

[0066] After testing: the viscosity is 0.58 dL / g, the slice b value is 5.5, the slice L value is 71, the diethylene glycol content is 1.52%, the terminal carboxyl content is 39.7 mol / t, and the molecular weight is 27546.

[0067] Example 5

[0068] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is replaced by 0.03% of the total mass of the mixed acid and ethylene glycol, i.e., 77.5 mg; the remaining steps and parameters remain the same.

[0069] After testing: the viscosity is 0.62dL / g, the slice b value is 5.0, the slice L value is 72, the diethylene glycol content is 1.18%, the terminal carboxyl content is 38.7mol / t, and the molecular weight is 25480.

[0070] Example 6

[0071] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is replaced by 0.1% of the total mass of the mixed acid and ethylene glycol, i.e., 258 mg; the other steps and parameters remain the same.

[0072] After testing: the viscosity is 0.71dL / g, the slice b value is 5.2, the slice L value is 75, the diethylene glycol content is 1.20, the terminal carboxyl content is 31.4mol / t, and the molecular weight is 26541.

[0073] Example 7

[0074] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the amount of a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is replaced by 0.7% of the total mass of the mixed acid and ethylene glycol, i.e., 1807.4 mg; the remaining steps and parameters remain the same.

[0075] After testing: the viscosity is 0.68dL / g, the slice b value is 6.7, the slice L value is 78, the diethylene glycol content is 1.36%, the terminal carboxyl content is 28.6mol / t, and the molecular weight is 35657.

[0076] Example 8

[0077] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate is replaced by a germanium-titanium composite catalyst obtained by compounding sodium germanate and tetraethyl titanate; the other steps and parameters remain the same.

[0078] After testing: the viscosity is 0.60dL / g, the slice b value is 6.1, the slice L value is 77, the content of diethylene glycol is 1.39%, the terminal carboxyl content is 34.3mol / t, and the molecular weight is 28640.

[0079] Example 9

[0080] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only a germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate is replaced by a germanium-titanium composite catalyst obtained by compounding tetrabutoxygermanium and titanium dioxide; the remaining steps and parameters remain the same.

[0081] After testing: the viscosity is 0.58 dL / g, the slice b value is 5.8, the slice L value is 73, the diethylene glycol content is 1.41%, the terminal carboxyl content is 36.5 mol / t, and the molecular weight is 26541.

[0082] Example 10

[0083] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the esterification reaction temperature is replaced from 210° C. to 185° C., and the other steps and parameters remain the same.

[0084] After testing: the viscosity is 0.70dL / g, the slice b value is 5.7, the slice L value is 83, the diethylene glycol content is 1.24%, the terminal carboxyl content is 27.7mol / t, and the molecular weight is 21541.

[0085] Embodiment 11

[0086] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the esterification reaction temperature is replaced from 210° C. to 230° C., and the other steps and parameters remain the same.

[0087] After testing: the viscosity is 0.63dL / g, the slice b value is 6.1, the slice L value is 78, the diethylene glycol content is 1.31%, the terminal carboxyl content is 36.7mol / t, and the molecular weight is 33764.

[0088] Example 12

[0089] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the esterification reaction time is replaced from 2 h to 3 h, and the other steps and parameters remain the same.

[0090] After testing: the viscosity is 0.76 dL / g, the slice b value is 5.2, the slice L value is 78, the diethylene glycol content is 1.42%, the terminal carboxyl content is 26.1 mol / t, and the molecular weight is 36475.

[0091] Embodiment 13

[0092] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction temperature is replaced from 245° C. to 230° C., and the other steps and parameters remain the same.

[0093] After testing: the viscosity is 0.66dL / g, the slice b value is 5.0, the slice L value is 82, the diethylene glycol content is 1.27%, the terminal carboxyl content is 31.6mol / t, and the molecular weight is 22643.

[0094] Embodiment 14

[0095] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction temperature is changed from 245° C. to 260° C., and the other steps and parameters remain the same.

[0096] After testing: the viscosity is 0.63dL / g, the slice b value is 6.8, the slice L value is 75, the diethylene glycol content is 1.33%, the terminal carboxyl content is 27.4mol / t, and the molecular weight is 29587.

[0097] Embodiment 15

[0098] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction time is replaced from 4 hours to 2 hours, and the other steps and parameters remain the same.

[0099] After testing: the viscosity is 0.73dL / g, the slice b value is 5.2, the slice L value is 71, the diethylene glycol content is 1.16%, the terminal carboxyl content is 29.9mol / t, and the molecular weight is 32527.

[0100] Example 16

[0101] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction time is changed from 4 hours to 5 hours, and the other steps and parameters remain the same.

[0102] After testing: the viscosity is 0.75 dL / g, the slice b value is 6.4, the slice L value is 82, the diethylene glycol content is 1.34%, the terminal carboxyl content is 29.8 mol / t, and the molecular weight is 35874.

[0103] Embodiment 17

[0104] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction time is changed from 4 hours to 6 hours, and the other steps and parameters remain the same.

[0105] After testing: the viscosity is 0.67dL / g, the slice b value is 6.8, the slice L value is 85, the diethylene glycol content is 1.46%, the terminal carboxyl content is 32.4mol / t, and the molecular weight is 33258.

[0106] Embodiment 18

[0107] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only the polycondensation reaction pressure is replaced from 50 Pa to 30 Pa, and the other steps and parameters remain the same.

[0108] After testing: the viscosity is 0.78dL / g, the slice b value is 5.0, the slice L value is 79, the diethylene glycol content is 1.24%, the terminal carboxyl content is 25.8mol / t, and the molecular weight is 37502.

[0109] Embodiment 19

[0110] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only ethylene glycol is replaced by an equimolar amount of 1,3-propylene glycol, that is, 99.3 g of ethylene glycol is replaced by 122 g of 1,3-propylene glycol; while ensuring that the amount of germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, and the amount of triphenyl phosphate is 0. .1%, the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of germanium titanium composite catalyst is 1404.5 mg, the amount of triphenyl phosphate is 280.9 mg, and the amount of antioxidant 1010 is 280.9 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-3,4-dimethylfuran-2,5-dicarboxylic acid propylene glycol copolyester, the structural formula is formula III:

[0111]

[0112] After testing: the viscosity is 0.76dL / g, the slice b value is 5.4, the slice L value is 80, the diethylene glycol content is 1.26, the terminal carboxyl content is 26.4mol / t, and the molecular weight is 38580.

[0113] Embodiment 20

[0114] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only ethylene glycol is replaced by an equimolar amount of 1,4-butanediol, that is, 99.3 g of ethylene glycol is replaced by 144 g of 1,4-butanediol; while ensuring that the amount of germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, and the amount of triphenyl phosphate is 1% of the total mass of the mixed acid and ethylene glycol. 0.1%, the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of germanium titanium composite catalyst is 1514.5 mg, the amount of triphenyl phosphate is 302.9 mg, and the amount of antioxidant 1010 is 302.9 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-3,4-dimethylfuran-2,5-dicarboxylic acid butanediol copolyester, the structural formula is Formula IV:

[0115]

[0116] After testing: the viscosity is 0.79dL / g, the slice b value is 5.2, the slice L value is 76, the diethylene glycol content is 1.24, the terminal carboxyl content is 26.3mol / t, and the molecular weight is 43627.

[0117] Embodiment 21

[0118] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with an equal molar amount of 2,3-dimethylterephthalic acid, that is, 18.4 g of 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with 19.4 g 2,3-dimethyl terephthalic acid; on the basis of ensuring that the amount of germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of germanium-titanium composite catalyst is 1296 mg, the amount of triphenyl phosphate is 259.2 mg, and the amount of antioxidant 1010 is 259.2 mg; the other steps and parameters remain the same; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-2,3-dimethyl terephthalate glycol copolyester, the structural formula of which is Formula V:

[0119]

[0120] After testing: the viscosity is 0.76dL / g, the slice b value is 5.9, the slice L value is 76, the diethylene glycol content is 1.41%, the terminal carboxyl content is 34.3mol / t, and the molecular weight is 36672.

[0121] Embodiment 22

[0122] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with an equal molar amount of 3,4-dimethylthiophene-2,5-dicarboxylic acid, that is, 18.4 g of 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with 20.0 g 3,4-dimethylthiophene-2,5-dicarboxylic acid; on the basis of ensuring that the amount of the germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1299 mg, the amount of triphenyl phosphate is 259.8 mg, and the amount of antioxidant 1010 is 259.8 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-3,4-dimethylthiophene-2,5-dicarboxylic acid ethylene glycol copolyester, the structural formula of which is Formula VI:

[0123]

[0124] After testing: the viscosity is 0.72dL / g, the slice b value is 5.4, the slice L value is 77, the diethylene glycol content is 1.30%, the terminal carboxyl content is 30.3mol / t, and the molecular weight is 35541.

[0125] Embodiment 23

[0126] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with an equal molar amount of 2,4,6-trimethylisophthalic acid, that is, 18.4 g of 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with 20.8 g 2,4,6-trimethylisophthalic acid; on the basis of ensuring that the amount of germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of germanium-titanium composite catalyst is 1303 mg, the amount of triphenyl phosphate is 260.6 mg, and the amount of antioxidant 1010 is 260.6 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-2,4,6-trimethylisophthalic acid ethylene glycol copolyester, the structural formula of which is Formula VII:

[0127]

[0128] After testing: the viscosity is 0.68dL / g, the slice b value is 6.3, the slice L value is 73, the diethylene glycol content is 1.48%, the terminal carboxyl content is 36.7mol / t, and the molecular weight is 36783.

[0129] Embodiment 24

[0130] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with an equal molar amount of 3,4-diphenylfuran-2,5-dicarboxylic acid, that is, 18.4 g of 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with 30.8 g 3,4-diphenylfuran-2,5-dicarboxylic acid; on the basis of ensuring that the amount of the germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1353 mg, the amount of triphenyl phosphate is 270.6 mg, and the amount of antioxidant 1010 is 270.6 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-3,4-diphenylfuran-2,5-dicarboxylic acid ethylene glycol copolyester, the structural formula of which is Formula VIII:

[0131]

[0132] After testing: the viscosity is 0.72dL / g, the slice b value is 6.8, the slice L value is 70, the diethylene glycol content is 1.36%, the terminal carboxyl content is 37mol / t, and the molecular weight is 36641.

[0133] Embodiment 25

[0134] A method for synthesizing 2,5-furandicarboxylic acid-based copolyester, which differs from Example 1 in that only 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with an equal molar amount of 3,4-diphenylthiophene-2,5-dicarboxylic acid, that is, 18.4 g of 3,4-dimethylfuran-2,5-dicarboxylic acid is replaced with 30.8 g 3,4-diphenylthiophene-2,5-dicarboxylic acid; on the basis of ensuring that the amount of the germanium-titanium composite catalyst obtained by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 is 0.5% of the total mass of the mixed acid and ethylene glycol, the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol, and the amount of antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol, the amount of the germanium-titanium composite catalyst is 1353 mg, the amount of triphenyl phosphate is 270.6 mg, and the amount of antioxidant 1010 is 270.6 mg; the other steps and parameters are kept consistent; the reaction is completed to obtain the product poly 2,5-furandicarboxylic acid-3,4-diphenylthiophene-2,5-dicarboxylic acid ethylene glycol copolyester, the structural formula of which is Formula IX:

[0135]

[0136] After testing: the viscosity is 0.78dL / g, the slice b value is 5.4, the slice L value is 72, the diethylene glycol content is 1.33%, the terminal carboxyl content is 26.5mol / t, and the molecular weight is 37897.

[0137] Embodiment 26

[0138] 0.7 mol FDCA (109.3 g) and 0.3 mol 3,4-dimethylfuran-2,5-dicarboxylic acid (55.2 g) were added to a slurry tank to obtain a mixed acid, and 1.6 mol ethylene glycol (EG 99.3 g) was simultaneously conveyed to the mixed acid through a pipeline. The mixed acid and ethylene glycol were fully mixed in the slurry tank and then entered into an esterification tank. The reaction was stopped at a pressure of 0.25 MPa and a temperature of 210° C. for 2 h to obtain a first intermediate and water, and the water was discharged;

[0139] The first intermediate is transported to a polycondensation kettle through a pipeline, a bypass is set on the pipeline from the esterification tank to the polycondensation kettle, 1320 mg of a germanium-titanium composite catalyst prepared by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 (the amount of the germanium-titanium composite catalyst is 0.5% of the total mass of the mixed acid and ethylene glycol), 264 mg of triphenyl phosphate (the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol) and 264 mg of an antioxidant 1010 (the amount of the antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol) are added, and the intermediate is put into the polycondensation kettle for melt polycondensation reaction, and the reaction is stopped after the reaction is carried out for 3 hours under the conditions of a pressure of 50 Pa and a temperature of 245° C. to obtain a product, poly-2,5-furandicarboxylic acid-3,4-dimethylfuran-2,5-dicarboxylic acid ethylene glycol copolyester.

[0140] After testing: the viscosity is 0.69 dL / g, the slice b value is 5.6, the slice L value is 75, the diethylene glycol content is 1.27%, the terminal carboxyl content is 26.7 mol / t, and the molecular weight is 30238.

[0141] Embodiment 27

[0142] 0.5 mol FDCA (78 g) and 0.5 mol 3,4-dimethylfuran-2,5-dicarboxylic acid (92.1 g) were added to a slurry tank to obtain a mixed acid, and 1.6 mol ethylene glycol (EG 99.3 g) was simultaneously conveyed to the mixed acid through a pipeline. The mixed acid and ethylene glycol were fully mixed in the slurry tank and then entered into an esterification tank. The reaction was stopped at a pressure of 0.25 MPa and a temperature of 210° C. for 2 h to obtain a first intermediate and water, and the water was discharged;

[0143] The first intermediate is transported to a polycondensation kettle through a pipeline, a bypass is set on the pipeline from the esterification tank to the polycondensation kettle, 1347 mg of a germanium-titanium composite catalyst prepared by compounding germanium oxide and tetrabutyl titanate in a mass ratio of 30:1 (the amount of the germanium-titanium composite catalyst is 0.5% of the total mass of the mixed acid and ethylene glycol), 269 mg of triphenyl phosphate (the amount of triphenyl phosphate is 0.1% of the total mass of the mixed acid and ethylene glycol) and 269 mg of an antioxidant 1010 (the amount of the antioxidant 1010 is 0.1% of the total mass of the mixed acid and ethylene glycol) are added, and the intermediate is put into the polycondensation kettle for melt polycondensation reaction, and the reaction is stopped after the reaction is carried out for 3 hours under the conditions of a pressure of 50 Pa and a temperature of 245° C. to obtain a product, poly-2,5-furandicarboxylic acid-3,4-dimethylfuran-2,5-dicarboxylic acid ethylene glycol copolyester.

[0144] After testing: the viscosity is 0.70dL / g, the slice b value is 5.7, the slice L value is 84, the diethylene glycol content is 1.28%, the terminal carboxyl content is 29.8mol / t, and the molecular weight is 35967.

[0145] The relevant experimental data statistics of Example 1 to Example 27 are shown in Table 1 to Table 8:

[0146] Table 1

[0147]

[0148] Table 2

[0149]

[0150] Table 3

[0151]

[0152] Table 4

[0153]

[0154] Table 5

[0155]

[0156]

[0157] Table 6

[0158]

[0159] Table 7

[0160]

[0161] Table 8

[0162]

[0163] The present invention uses complementary pressure decay adsorption and permeation technology to study the gas barrier properties of FDCA-based copolyesters. For the sake of comparison, conventional polymers with good gas barrier properties, such as PET, are used as controls. The barrier improvement factor BIF represents the permeability coefficient of the gas in PET divided by the permeability coefficient of the gas in the TDCA-based copolyester film. The higher the BIFP, the better the gas barrier properties of the measured material. The barrier test data of some embodiments are shown in Tables 9 and 10:

[0164] Table 9

[0165] serial number T(℃) <![CDATA[P O2 (Sweep) a ]]> <![CDATA[BIF O2 b ]]> <![CDATA[P CO2 (Sweep) c ]]> <![CDATA[BIF CO2 d ]]> PET 35 0.114 1 0.49 1 PEF 35 0.011 11 0.026 19 Example 1 35 0.0067 17 0.021 23 Embodiment 21 35 0.0076 15 0.023 21 Embodiment 22 35 0.006 19 0.019 26 Embodiment 23 35 0.0054 21 0.016 29 Embodiment 24 35 0.0045 25 0.014 35 Embodiment 25 35 0.004 27 0.012 39

[0166] Note: a. Oxygen permeability coefficient 1 barrer = 10 -10 cm 3 cm / cm 2 ·s·cmHg; b. oxygen barrier improvement factor; c. carbon dioxide permeability coefficient; d. carbon dioxide barrier improvement factor.

[0167] Table 10

[0168]

[0169]

[0170] Note: e. Water permeability coefficient; f. Water barrier improvement factor

[0171] The present invention also studies the mechanical properties of polyester, and the test data of some embodiments are shown in Table 11:

[0172] Table 11

[0173]

[0174] In summary, the present invention uses FDCA, dibasic acid and diol as raw materials, and prepares FDCA-based copolyester through esterification and polycondensation reaction under the action of catalysts, antioxidants, stabilizers and other additives. The copolyester synthesized by the present invention has a low terminal carboxyl content and good properties comparable to PET, and can be widely used in the fields of fiber, film, packaging, etc.

[0175] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0176] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A 2,5-furandicarboxylic acid-based copolyester, characterized in that: A compound of formula I: Where Ar is R is one of -H, alkyl, and aryl, and R cannot be -H at the same time; n is an integer between 2 and 10; x and y are average polymerization degrees, x=1-150; y=1-150.

2. A method for synthesizing 2,5-furandicarboxylic acid-based copolyester as claimed in claim 1, characterized in that: The following steps are involved: 2,5-furandicarboxylic acid and a dibasic acid are mixed in a molar ratio of 1:0.1-1 to obtain a mixed acid, and a diol is added to the mixed acid for esterification reaction to generate a first intermediate and water; a germanium-titanium composite catalyst, an antioxidant and a phosphorus stabilizer are added to the first intermediate for melt polycondensation reaction to obtain a 2,5-furandicarboxylic acid-based copolyester.

3. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The dibasic acid is Wherein, R is one of -H, alkyl, and aryl, and R cannot be -H at the same time.

4. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The diol includes ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol or 1,8-octanediol.

5. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The ratio of the total molar amount of the dibasic acid and 2,5-furandicarboxylic acid to the molar amount of the diol in the mixed acid is 1:1.05-2.

0.

6. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The germanium-titanium composite catalyst is compounded by mixing a germanium-based catalyst and a titanium-based catalyst in a mass ratio of 20-50:1; The amount of the germanium-titanium composite catalyst used is 0.01%-1% of the total mass of FDCA, dibasic acid and diol.

7. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The amount of the antioxidant is 0.01%-0.2% of the total mass of FDCA, dibasic acid and diol; The antioxidant includes antioxidant 1010, antioxidant 1178, antioxidant 1076, antioxidant 618, antioxidant 425, antioxidant 330, antioxidant 626 or antioxidant 168.

8. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The amount of the phosphorus stabilizer is 0.01%-0.2% of the total mass of FDCA, dibasic acid and diol; The phosphorus-based stabilizer includes triphenyl phosphate, triphenyl phosphite, ethyl phosphate, phosphoric acid, trimethyl phosphate, trimethyl phosphite or polyphosphoric acid.

9. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The temperature of the esterification reaction is 185-235° C., the reaction time is 70-200 min, and the reaction pressure is 0.1-0.25 MPa.

10. The method for synthesizing 2,5-furandicarboxylic acid-based copolyester according to claim 2, characterized in that: The temperature of the polycondensation reaction is 230-265° C., the reaction time is 120-360 min, and the reaction pressure is 1-100 Pa.

Citation Information

Cited By

  • Furan polyester composition and use thereof

    WO2026108962A1