Photocurable organopolysiloxane, photocurable organopolysiloxane composition, and cured product

By adjusting the amount of polymerizable functional groups and alkoxysilyl groups, increasing the T-unit ratio of photocurable organopolysiloxane, the deficiencies in durability and reprocessability of the polysiloxane resin are solved, and coating is achieved The fabric and durability are greatly improved and are suitable for a variety of materials and process needs.

CN118994582APending Publication Date: 2024-11-22DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410284587.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-03-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing photocurable polysiloxane resins have shortcomings in durability and reprocessability, and it is difficult to meet the needs of reuse of solar panels and the shape adjustment of resist films in the photolithography process.

Method used

By adjusting the T unit ratio, the amount of polymerizable functional groups and alkoxysilyl groups, it is ensured that the proportion of T units in the photocurable organopolysiloxane accounts for more than 70 mol % of the total silanoxy units, and the content of polymerizable functional groups is greater than 70 mol %. A silane group is added in the range of 0.1 to 10 mass % to improve the durability and reprocessability of the hardened product.

Benefits of technology

The hardened material has achieved excellent coating properties, durability and reprocessing properties, and is suitable for a variety of application scenarios, such as efficient peeling and reformation of resist films in electronic materials and photolithography processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004738683370000021
    Figure BDA0004738683370000021
  • Figure BDA0004738683370000071
    Figure BDA0004738683370000071
  • Figure BDA0004738683370000181
    Figure BDA0004738683370000181
Patent Text Reader

Abstract

The invention provides a photo-curable organopolysiloxane, a photo-curable organopolysiloxane composition and a cured product, wherein the photo-curable organopolysiloxane, the photo-curable organopolysiloxane composition and the cured product are excellent in coating property, durability of the obtained cured product and reprocessing property. A photo-curable organopolysiloxane having a polymerizable functional group represented by *-O-R11-Y (Y is a group containing a carbon-carbon unsaturated bond, and * represents a bonding position with a silicon atom of the organopolysiloxane) and an alkoxysilyl group, the photo-curable organopolysiloxane being characterized in that: the alkoxysilyl group is an alkoxysilyl group; the ratio of the T units in the total siloxy units is 70 mol% or more, and the photocurable organopolysiloxane contains 40 mass% or more of the polymerizable functional groups and contains 0.1 mass% to 10 mass% of the alkoxysilyl groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photocurable organopolysiloxane, a photocurable organopolysiloxane composition and a cured product. Background Art

[0002] Photocurable polysiloxanes can be used in a wide range of applications such as coating materials, adhesive materials, packaging materials, and electronic materials because the composition containing the photocurable polysiloxane itself has excellent coating properties (fluidity) and the obtained cured product also has excellent durability.

[0003] Specific uses of photocurable polysiloxane include protective coating agents for light emitting diodes (LEDs) or solar panels (for example, Patent Document 1), and base polymers for photoresists (for example, Patent Documents 2 and 3).

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] [Patent Document 1] Japanese Patent Publication No. 2015-516478

[0007] [Patent Document 2] Japanese Patent Publication No. 2011-23698

[0008] [Patent Document 3] WO2016 / 072202 Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] The "reprocessability" of the polysiloxane resin that can be easily cleaned after curing is an important required performance. In the case of the above-mentioned application, in addition to the need to remove the protective coating agent when reusing the panel after years of degradation in the solar panel, when the pattern shape of the resist film formed in the photolithography process is not the desired shape, the resist film is peeled off and the resist film is formed again.

[0011] The polysiloxane resins disclosed in Patent Documents 1 to 3 are not said to have sufficient durability and reprocessability, and therefore a polysiloxane resin having excellent reprocessability is desired.

[0012] An object of the present invention is to provide a photocurable organopolysiloxane having excellent durability and reworkability of the obtained cured product.

[0013] Another problem to be solved by the present invention is to provide a cured product of a composition containing a photocurable organopolysiloxane having excellent durability and reworkability.

[0014] [Technical means to solve the problem]

[0015] The present inventors have conducted intensive studies to solve the above problems and have found that an organopolysiloxane having a ratio of T units, a polymerizable functional group, and an amount of alkoxysilyl groups within specific ranges can provide a cured product having excellent durability and reworkability, thereby completing the present invention.

[0016] That is, the present invention relates to a photocurable organopolysiloxane and the like.

[0017] 1. A photocurable organopolysiloxane having a polymerizable functional group represented by the following general formula (1) and an alkoxysilane group, wherein:

[0018] The proportion of T units in the total siloxy units is 70 mol% or more,

[0019] The photocurable organopolysiloxane contains 40% by mass or more of the polymerizable functional group represented by the general formula (1), and contains the alkoxysilyl group in a range of 0.1% by mass to 10% by mass.

[0020] [Chemistry 3]

[0021] *-OR 11 -Y (1)

[0023] (In the general formula (1),

[0024] R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms,

[0025] Y is a group containing a carbon-carbon unsaturated bond,

[0026] * indicates the bonding position with the silicon atom of the organopolysiloxane)

[0027] 2. The photocurable organopolysiloxane according to 1, wherein the polymerizable functional group represented by the general formula (1) is a polymerizable functional group represented by the following general formula (1-2).

[0028] [Chemistry 4]

[0029]

[0030] (In the general formula (1-2),

[0031] R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms,

[0032] R 12is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms,

[0033] * indicates the bonding position with the silicon atom of the organopolysiloxane)

[0034] 3. The photocurable organopolysiloxane according to 1 or 2, wherein the content of the polysiloxane structure is 35% by mass or more.

[0035] 4. The photocurable organopolysiloxane according to any one of 1 to 3, wherein the viscosity at 25° C. is 150 mPa·s or less.

[0036] 5. A photocurable organopolysiloxane composition comprising the photocurable organopolysiloxane according to any one of 1 to 4 and a photopolymerization initiator.

[0037] 6. The photocurable organopolysiloxane composition according to 5, which is a resist composition.

[0038] 7. A cured product, which is a cured product of the photocurable organopolysiloxane composition according to 5 or 6.

[0039] [Effects of the Invention]

[0040] According to the present invention, there is provided a photocurable organopolysiloxane having excellent coating properties and excellent durability and reworkability of the obtained cured product.

[0041] According to the present invention, a cured product of a composition containing a photocurable organopolysiloxane having excellent durability and reworkability can be provided. DETAILED DESCRIPTION

[0042] Hereinafter, an embodiment of the present invention will be described. The present invention is not limited to the following embodiment, and can be implemented with appropriate modifications within a range that does not impair the effects of the present invention.

[0043] Furthermore, the compounds in this specification may be derived from fossil resources or biological resources.

[0044] [Photocurable organopolysiloxane]

[0045] The photocurable organopolysiloxane of the present invention has a polymerizable functional group represented by the following general formula (1) and an alkoxysilyl group, contains 40% by mass or more of the polymerizable functional group represented by the general formula (1), and contains the alkoxysilyl group in a range of 0.1% by mass to 10% by mass.

[0046] [Chemistry 5]

[0047] *-OR 11 -Y (1)

[0049] (In the general formula (1),

[0050] R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms,

[0051] Y is a group containing a carbon-carbon unsaturated bond,

[0052] * indicates the bonding position with the silicon atom of the organopolysiloxane)

[0053] In the present invention, by setting the amount of alkoxysilyl groups in the organopolysiloxane to a specific range, setting the amount of specific polymerizable functional groups to a certain level or more, and setting the ratio of T units in the organopolysiloxane to a certain level or more in the total siloxy units, the coating properties of the composition itself and the durability and reworkability of the obtained cured product can be improved.

[0054] The bonding part of the polymerizable functional group represented by the general formula (1) is degradable. It is presumed that when the organopolysiloxane is treated with an acid or an alkali, the bonding part of the polymerizable functional group will decompose, thereby collapsing the cross-linked structure of the organopolysiloxane and making it possible to wash it. Therefore, by having a certain amount of the polymerizable functional group represented by the general formula (1), reprocessability can be ensured.

[0055] In the general formula (1), examples of the group containing a carbon-carbon unsaturated bond represented by Y include a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acrylamido group, a vinyl ether group, an allyl group, a styryl group, and a maleimide group.

[0056] As R 11 Examples of the alkylene group having 1 to 12 carbon atoms include methylene, ethylene, n-propylene, n-butylene, n-pentylene, n-hexylene, n-heptylene, n-octylene, n-nonylene, n-decylene, n-dodecylene, isopropylene, 2-methylpropylene, 2-methylhexylene, and tetramethylethylene.

[0057] As R 11 The alkylene group having 1 to 12 carbon atoms is preferably an alkylene group having 1 to 5 carbon atoms, and more preferably a methylene group, an ethylene group, a n-propylene group or an isopropylene group.

[0058] As R 11 In the alkylene group having 1 to 12 carbon atoms, a part of -CH2- may be replaced by a carbonyl group (-C(=O)-), an ether bond (-O-), a phenylene group, an amide bond or a carbamate bond, and a hydroxyl group or the like may further substitute on the carbon atom.

[0059] The upper limit of the amount of the polymerizable functional groups in the photocurable organopolysiloxane of the present invention is not particularly limited, and is, for example, 80% by mass or less, 60% by mass or less, or 50% by mass or less.

[0060] The alkoxysilyl group is hydrolyzed by treatment with an acid or an alkali to form a silanol group, thereby improving the cleaning property of the organopolysiloxane. Therefore, by having a certain amount of alkoxysilyl groups, reprocessability can be ensured.

[0061] The content of the alkoxysilyl group in the photocurable organopolysiloxane of the present invention is in the range of 0.1% by mass to 10% by mass, preferably in the range of 0.1% by mass to 8.0% by mass, and more preferably in the range of 0.1% by mass to 6.0% by mass.

[0062] The alkoxysilyl group contained in the photocurable organopolysiloxane of the present invention is preferably an alkoxysilyl group represented by the following general formula (2).

[0063] [Chemistry 6]

[0064] *-OR 21 (2)

[0066] (In the general formula (2),

[0067] R 21 is an alkyl group having 1 to 12 carbon atoms,

[0068] * indicates the bonding position with the silicon atom of the organopolysiloxane)

[0069] As R 21 The alkyl group having 1 to 12 carbon atoms is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0070] As R 21 The alkyl group does not contain a carbon-carbon unsaturated bond. 21 The alkyl group may further have a substituent such as a halogen atom, a hydroxyl group, a cyano group, or an amino group.

[0071] The amounts of the polymerizable functional groups and alkoxysilyl groups in the photocurable organopolysiloxane of the present invention are confirmed by the method described in Examples.

[0072] The silaneoxy unit has R3SiO 1 / 2 Unit (M unit), SiO 4 / 2 Unit (Q unit), R2SiO 2 / 2 Unit (D unit) and RSiO 3 / 2Units (T units) (R is a hydrogen atom or an aliphatic hydrocarbon group), and the ratio of T units in the total siloxy units in the photocurable organopolysiloxane of the present invention is 70 mol% or more. When the ratio of T units is 70 mol% or more, a photocurable organopolysiloxane that can achieve both the coating properties of the composition and the durability and reprocessability of the obtained cured product can be obtained.

[0073] The ratio of each siloxy unit in the photocurable organopolysiloxane is confirmed by the method described in Examples.

[0074] The upper limit of the ratio of the T unit in the photocurable organopolysiloxane of the present invention is not particularly limited, and may be, for example, 100 mol % or less.

[0075] The aliphatic hydrocarbon group as R in the siloxy unit is, for example, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a phenyl group, or a phenoxy group.

[0076] The number average molecular weight of the photocurable organopolysiloxane of the present invention is preferably in the range of 500 to 5,000.

[0077] The number average molecular weight of the photocurable organopolysiloxane can be confirmed by gel permeation chromatography (GPC).

[0078] From the viewpoint of improving the durability and weather resistance of the cured product, the content of the polysiloxane structure in the photocurable organopolysiloxane of the present invention is preferably 35% by mass or more, more preferably 50% by mass or more.

[0079] In addition, the so-called "polysiloxane structure" refers to a repeating structure represented by "Si-O-Si". The upper limit of the content of the polysiloxane structure is not particularly limited, and is, for example, 60% by mass or less or 70% by mass or less.

[0080] The content of the polysiloxane structure in the photocurable organopolysiloxane is confirmed by the method described in Examples.

[0081] When a composition containing photocurable polysiloxane is used as a coating material for electronic devices, the coating properties of the composition containing photocurable polysiloxane become an important performance. When a composition whose viscosity is reduced by dilution with a solvent is used for electronic device coating, there is a concern that the volatile components of the solvent may cause corrosion or degradation of electrical / electronic parts and circuit substrates on which they are mounted. Therefore, it is required to have a coating viscosity suitable for following the fine uneven surfaces of electronic parts or radiator surfaces using only photocurable polysiloxane.

[0082] The photocurable organopolysiloxane of the present invention can exhibit coating properties to such an extent that it can follow the fine uneven surfaces of the electronic component or heat sink surface only by using the resin.

[0083] The viscosity of the photocurable organopolysiloxane of the present invention is preferably 150 mPa·s or less, and more preferably 100 mPa·s or less. The lower limit of the viscosity is not particularly limited, and is, for example, 10 mPa·s or more.

[0084] The viscosity of the photocurable organopolysiloxane can be confirmed by the method described in Examples.

[0085] The photocurable organopolysiloxane of the present invention is preferably a compound in which a group Y including a carbon-carbon unsaturated bond is linked to a silicon atom through a bond represented by Si-ORY, and the silicon atom is a part of a silicone oligomer.

[0086] Likewise, the photocurable organopolysiloxane of the present invention is preferably a compound in which the silicon atom of the alkoxysilyl group is a part of a silicone oligomer.

[0087] The synthesis of the photocurable organopolysiloxane of the present invention is not particularly limited, and known conventional methods can be used. For example, the following methods can be cited: using a compound having a polymerizable unsaturated group and a hydroxyl group as a raw material and synthesizing it with a chlorosilane compound through a dehydrochlorination reaction; or synthesizing it with an alkoxysilane compound through an ester exchange; or reacting it with a hydrosilane compound using a Lewis acid catalyst such as a boron compound.

[0088] The photocurable organopolysiloxane of the present invention is preferably a compound containing a silicone oligomer having an alkoxysilyl group and a compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond as reaction components.

[0089] Here, the “reaction component” refers to a component constituting the structure of the photocurable organopolysiloxane, and a solvent, a catalyst, etc. that do not constitute the structure are not included in the “reaction component”.

[0090] The silicone oligomer having an alkoxysilyl group can be prepared by a known polycondensation reaction using a hydrolyzable alkoxysilane compound as a reaction component.

[0091] The hydrolyzable alkoxysilane compound used may be one alone or two or more. By adjusting the type and amount of the hydrolyzable alkoxysilane compound, the ratio of T units, the content of polysiloxane structure, the amount of alkoxysilane groups, etc. of the obtained photocurable organopolysiloxane can be adjusted.

[0092] As the silicone oligomer having an alkoxysilyl group used in the production of the photocurable organopolysiloxane, a commercially available product can be used.

[0093] The compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond is preferably a (meth)acrylate compound having a hydroxyl group. In this case, the polymerizable functional group in the organopolysiloxane is, for example, a functional group represented by the following general formula (1-2).

[0094] [Chemistry 7]

[0095]

[0096] (In the general formula (1-2),

[0097] R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms,

[0098] R 12 is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms,

[0099] * indicates the bonding position with the silicon atom of the organopolysiloxane)

[0100] In the general formula (1) and the general formula (1-2), R 11 The alkylene group having 1 to 12 carbon atoms is preferably an alkylene group having 1 to 5 carbon atoms, and R 12 Preferred is a hydrogen atom or a methyl group.

[0101] The (meth)acrylate compound having a hydroxyl group is preferably a compound in which the “*” portion of the functional group represented by the general formula (1-2) is a hydrogen atom.

[0102] Specific examples of the (meth)acrylate compound having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, tricyclodecane dimethanol acrylate, adamantanediol acrylate, β-carboxyethyl acrylate, pentaerythritol triacrylate, and the like.

[0103] The (meth)acrylate compound having a hydroxyl group may be used alone or in combination of two or more.

[0104] There is no particular limitation on the method for producing the photocurable organopolysiloxane, and the photocurable organopolysiloxane can be produced by the method described above. As a particularly convenient production method, the reaction of a silicone oligomer having an alkoxysilyl group with a compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond can be carried out, for example, by heating in the presence of an acid catalyst (e.g., sulfuric acid).

[0105] Here, the photocurable organopolysiloxane of the present invention can be produced by making the alkoxysilyl group equivalent of the silicone oligomer excessive compared to the hydroxyl group equivalent of the compound having a hydroxyl group and a polymerizable group.

[0106] [Photocurable organopolysiloxane composition]

[0107] The photocurable organopolysiloxane of the present invention can be suitably used as a base polymer of the photocurable organopolysiloxane composition of the present invention (hereinafter sometimes simply referred to as "the composition of the present invention") which has excellent coating properties and the obtained cured product has excellent durability and reworkability.

[0108] The content of the photocurable organopolysiloxane of the present invention in the composition of the present invention is, for example, 80% by mass or more, and preferably 90% by mass or more, based on the solid content in the composition.

[0109] Here, the "solid content" refers to the total amount of components excluding a solvent described later from the total amount of the composition.

[0110] The composition of the present invention contains the photocurable organopolysiloxane of the present invention and a photopolymerization initiator.

[0111] The photopolymerization initiator may be a substance that absorbs the light source used for photocuring, and examples thereof include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinopropane-1-one, 1-Butanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane, 1,2-octanedione, 1-[4-(phenylthio)-,2-(O-benzoyl oxime)], 2-hydroxy-2-methyl-1-phenyl-propane-1-one, methyl phenylglyoxylate, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc.

[0112] As the photopolymerization initiator, commercially available products can be used, and examples thereof include OMNIRAD 1000, OMNIRAD 248, OMNIRAD 481, OMNIRAD 4817, OMNIRAD 4MBZ-flakes, OMNIRAD 500, OMNIRAD 659, OMNIRAD 73, OMNIRAD 784, OMNIRAD 81, OMNIRAD BDK, OMNIRAD MBS, OMNIRAD BP-flakes, and OMNIRAD BP-flakes. BP-flakes), OMNIRAD DETX, OMNIRAD EDB, OMNIRAD EHA, OMNIRAD EMK, OMNIRAD ITX, OMNIRAD MBF, OMNIRAD OMBB, OMNIRAD TPO, OMNIRAD )410、OMNIRAD BL723、OMNIRAD BL724、OMNIRAD BL750、OMNIRAD BL751、OMNIRAD 1173、OMNIRAD 127、OMNIRAD 184、OMNIRAD 184FF、OMNIRAD OMNIRAD 2022、OMNIRAD 2100、OMNIRAD 2959、OMNIRAD 369、OMNIRAD 369E、OMNIRAD 379、OMNIRAD 379EG、OMNIRAD 4265、OMNIRAD 754、OMNIRAD AD)819, OMNIRAD819DW, OMNIRAD907, OMNIRAD907FF, OMNIRADBP, OMNIRAD127D, ESACURE1001M, ESACUREONE, ESACUREA198, ESACUREKIP160, ESACUREKIP150, ESACURE KIP100F, ESACURE KIP-LT, ESACURE KIP-IT, ESACURE KTO-46, ESACURE DP-250, ESACURE TZT, ESACURE KT-55 (manufactured by IGM), etc.

[0113] The content of the photopolymerization initiator in the composition of the present invention is in the range of, for example, 0.01 parts by mass to 10 parts by mass, or preferably 0.1 parts by mass to 5 parts by mass, relative to 100 parts by mass of the photocurable organopolysiloxane.

[0114] The compositions of the present invention may also contain a polymerization inhibitor.

[0115] The polymerization inhibitor may be a known polymerization inhibitor, for example, hydroquinone, p-methoxyphenol, di-tert-butyl-p-cresol, pyrogallol, tert-butylcatechol, benzoquinone, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), N-nitrosophenylhydroxylamine salts (for example, ammonium salts, cerous salts), etc.

[0116] The content of the photopolymerization initiator in the composition of the present invention is, for example, in the range of 0.001 to 1 part by mass, or preferably in the range of 0.01 to 0.5 parts by mass, relative to 100 parts by mass of the photocurable organopolysiloxane of the present invention.

[0117] The composition of the present invention may contain a solvent. By adding a solvent, the viscosity of the composition or the coating film thickness can be adjusted.

[0118] As the solvent, for example, the following can be used: aliphatic or alicyclic hydrocarbons such as n-hexane, n-heptane, n-octane, cyclohexane, and cyclopentane; aromatic hydrocarbons such as toluene, xylene, ethylbenzene, and anisole; alcohols such as methanol, ethanol, n-butanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; esters such as ethyl acetate, n-butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alkyl ethers; ethers such as 1,2-dimethoxyethane, tetrahydrofuran, and dioxane; N-methylpyrrolidone, dimethylformamide, and dimethylacetamide.

[0119] The content of the solvent in the composition of the present invention is not particularly limited and can be appropriately set according to the target viscosity or coating film thickness.

[0120] The compositions of the present invention may also contain a surfactant.

[0121] As the surfactant, any of nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants can be used, but nonionic surfactants are preferred.

[0122] Examples of the nonionic surfactant include polyoxyalkylene alkyl ether surfactants, polyoxyalkylene fatty acid ester surfactants, sorbitan fatty acid ester surfactants, polyoxyalkylene alkylamine surfactants, Pluronic (registered trademark) (triblock copolymer of polyethylene oxide and polypropylene oxide) surfactants, fluorine-based surfactants, silicone-based surfactants, and acrylic acid polymerization-based surfactants.

[0123] Examples of the anionic surfactant include alkylbenzene sulfonate surfactants, alkyl alcohol sulfate ester surfactants, polyoxyalkylene alkyl ether sulfate surfactants, alkyl alcohol phosphate ester surfactants, polyoxyalkylene alkyl ether phosphate surfactants, polyoxyalkylene alkyl ether acetate surfactants, and fluorine-based surfactants. Either an acid type or a neutralized type may be used.

[0124] Examples of the cationic surfactant include tetraalkylammonium halide surfactants, alkylpyridinium halide surfactants, and alkylimidazoline halide surfactants.

[0125] Examples of the amphoteric surfactant include alkyl betaine-based surfactants, alkyl imidazolinium betaine-based surfactants, and lecithin-based surfactants.

[0126] The content of the surfactant in the composition of the present invention is, for example, in the range of 0.001 to 10 parts by mass, preferably in the range of 0.01 to 8 parts by mass, and more preferably in the range of 0.1 to 5 parts by mass, relative to 100 parts by mass of the photocurable organopolysiloxane of the present invention.

[0127] The composition of the present invention may also be formulated with other ingredients within the scope of not impairing the effects of the present invention. Examples of other ingredients include organic pigments, inorganic pigments, extender pigments, organic fillers, inorganic fillers, photosensitizers, ultraviolet absorbers, antioxidants, and adhesion aids.

[0128] The composition of the present invention can exhibit sufficient coating properties only with the resin by controlling the terminal functional group and molecular weight of the photocurable organopolysiloxane.

[0129] In Japanese Patent Application Laid-Open No. 2011-23698, an alkoxysilane compound is added to improve the coating properties of a silicone polymer. However, in the present invention, since the photocurable organopolysiloxane itself has good fluidity, there is no need to add a low molecular weight alkoxysilane compound.

[0130] As mentioned above, although the components in the photocurable organopolysiloxane composition of the present invention are described, each component may be used alone or in combination of two or more.

[0131] The photocurable organopolysiloxane composition of the present invention is a photocurable composition that can be cured by irradiation with light. For example, the photocurable organopolysiloxane composition of the present invention is applied on a substrate to form a coating film, and the coating film is irradiated with light to form a cured layer on the substrate.

[0132] The substrate can be appropriately selected according to the purpose, and examples thereof include quartz, sapphire, glass, plastic, ceramic material, vapor-deposited film (chemical vapor deposition (CVD), physical vapor deposition (PVD), sputtering), magnetic film, reflective film, metal substrates such as Ni, Cu, Cr, Fe, stainless steel, paper, spin-on glass (SOG), spin-on carbon (SOC), polymer substrates such as polyester film, polycarbonate film, polyimide film, thin film transistor (TFT) array substrate, electrode plate of plasma display panel (PDP), conductive substrates such as indium tin oxide (ITO) or metal, insulating substrates, semiconductor manufacturing substrates such as silicon, silicon nitride, polycrystalline silicon, silicon oxide, amorphous silicon, etc.

[0133] In addition, the shape of the substrate is not particularly limited, and can be any shape corresponding to the purpose, such as a flat plate, a sheet, or a shape having curvature on the entire surface or a portion of a three-dimensional shape. In addition, the hardness and thickness of the substrate are also not limited.

[0134] As a coating method of the photocurable organopolysiloxane composition of the present invention, various methods such as spray coating, spin coating, dipping, roll coating, blade coating, doctor roll coating, doctor blade coating, curtain coating, slit coating, screen printing, and inkjet coating can be used.

[0135] The spin coating method is preferred because a coating film having good in-plane uniformity of film thickness can be obtained.

[0136] Examples of light sources for irradiation include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, carbon arcs, mercury-xenon lamps, excimer lasers (XeCl, KrF, ArF, etc.), ultraviolet lasers or visible light lasers, ultraviolet LEDs or visible light LEDs, etc.

[0137] The amount of light irradiation can be set appropriately, for example, 10 mJ / cm 2 ~10000mJ / cm 2 range.

[0138] A baking step of heating the substrate after coating the photocurable organopolysiloxane composition and before light irradiation may be provided. Various methods such as proximity method, adsorption method, conveyor method, induction heating using microwaves, etc. may be used as the baking method, and these methods may also be combined.

[0139] The baking conditions are not particularly limited, but for example, the baking temperature is in the range of 70° C. to 180° C., and the baking time is in the range of 0.3 minutes to 10 minutes.

[0140] When the photocurable organopolysiloxane composition of the present invention is used for photoimprinting, a mold having a pattern formed in advance is pressed against a coating film of the photocurable organopolysiloxane composition formed on the substrate, and light is irradiated to cure the coating film while the mold is in contact, thereby obtaining a cured film having a pattern formed thereon.

[0141] In addition, the baking step may be performed before the molds are brought into contact with each other, or may be performed after the molds are pressed.

[0142] Regarding the material of the optical imprinting mold, as a light-transmitting material, there can be listed: quartz, ultraviolet light-transmitting glass, sapphire, diamond, silicone materials such as polydimethylsiloxane, fluororesins, cycloolefin resins, other light-transmitting resin materials, etc. In addition, if the substrate used is a light-transmitting material, the imprinting mold can also be a light-impermeable material. As a light-impermeable material, metal, SiC, mica, etc. can be listed. Among them, in terms of allowing ultraviolet rays to be well transmitted, high hardness, and high surface smoothness, a quartz mold is particularly preferred.

[0143] The mold for photoimprinting can be selected from molds of any shape such as a flat surface, a belt, a roll, or a roll-belt shape.

[0144] The mold for photoimprinting may be a mold subjected to a release treatment to improve the releasability between the photocurable composition and the mold surface. Examples of the release treatment include treatment with a silicone silane coupling agent or a fluorine silane coupling agent.

[0145] Regarding the method of irradiating light, when the mold is made of a light-transmitting material, a method of irradiating light from the mold side can be adopted, and when the substrate is made of a light-transmitting material, a method of irradiating light from the substrate side can be adopted.

[0146] If there is a concern about the followability of the formed pattern, it may be heated to a temperature at which sufficient fluidity can be obtained during light irradiation. The temperature during heating is preferably 0°C to 300°C, more preferably 0°C to 200°C, further preferably 0°C to 150°C, and particularly preferably 25°C to 80°C. Within the temperature range, the pattern shape formed by the photocurable composition can be maintained with good accuracy.

[0147] After curing, the mold is demolded to obtain a cured film having a convex-concave pattern that is a transfer of the concave-convex pattern of the mold. In order to suppress deformation such as warping of the substrate or to improve the accuracy of the concave-convex pattern, the peeling step is preferably performed after the temperature of the cured film is lowered to near room temperature (25°C).

[0148] After demolding the mold, if there is any residue of the cured product in the mold, it can be cleaned with a cleaning solution. Since the mold is reused, if there is any residue of the cured product in the mold, there is a concern that it may adversely affect pattern formation.

[0149] The photocurable organopolysiloxane contained in the photocurable organopolysiloxane composition of the present invention contains a large amount of Si-OR 11 -Y represented by a polymerizable functional group, wherein the Si-OR 11 Since the part is highly decomposable by the cleaning liquid, the photocurable organopolysiloxane composition of the present invention is excellent in reprocessability.

[0150] The cleaning liquid used in cleaning the mold can be selected appropriately according to the material of the mold, and both acid cleaning liquid and alkaline cleaning liquid can be used.

[0151] Examples of the acid cleaning liquid include sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, acetic acid, phosphoric acid, aqua regia, dilute hydrofluoric acid, sulfuric acid hydrogen peroxide, hydrochloric acid hydrogen peroxide, and the like. Examples of the alkaline cleaning liquid include not only caustic soda, caustic potash, and other caustic alkalis, or various inorganic alkalis such as silicates, phosphates, and carbonates, but also organic alkalis such as tetramethylammonium hydroxide, ammonia water, ammonia hydrogen water, and ammonia hydrogen peroxide.

[0152] There is a concern that the alkaline cleaning solution may dissolve SiO2, so when the mold is glass or quartz, an acid cleaning solution is preferred, and sulfuric acid hydrogen peroxide is particularly preferred. In particular, when cleaning a quartz mold having a fine pattern of less than 100 nm, there is a concern that the rectangularity of the mold may be damaged due to the dissolution of SiO2 in the alkaline cleaning solution, so by using an acid cleaning solution, the mold can be cleaned without damaging the fine pattern and can be reused.

[0153] The cleaning method is not particularly limited, and examples thereof include spraying, showering, immersion, heated immersion, ultrasonic immersion, rotation, bubbling, shaking, brushing, steaming, grinding, and the like. In order to prevent the re-adhesion of the cleaned contaminants, the rotation method is particularly preferred.

[0154] The laminate produced using the photocurable organopolysiloxane composition of the present invention can be formed by coating a resist material on a substrate and immediately curing it to form a resist film, or by peeling off a resist film formed on a temporary substrate and attaching it to a substrate to form a laminate. If a pattern is formed on the resist film, dry etching the laminate to obtain a patterned product in which the pattern is transferred to the substrate by dry etching.

[0155] As the gas used in dry etching, any known gas can be used, for example, oxygen, carbon monoxide, carbon dioxide and other oxygen atom-containing gases, helium, nitrogen, argon and other inactive gases, chlorine, boron trichloride and other chlorine-based gases, fluorine, fluorocarbon-based gases, hydrogen, ammonia, etc. These gases can be used alone or in a suitable mixture.

[0156] By performing etching using these etching gases, a desired pattern can be formed on the substrate.

[0157] [Example]

[0158] Hereinafter, the present invention will be specifically described by way of Examples and Comparative Examples.

[0159] In addition, the present invention is not limited to the following examples.

[0160] In the production of the photocurable organopolysiloxane described below, a silicone oligomer having an alkoxysilyl group described below is used.

[0161] Alkoxysilane compound (a-1): "KR-500" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer raw material, viscosity: 25 mPa·s, methoxy group content: 28 mass %

[0162] Alkoxysilane compound (a-2): "X-40-9225" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer raw material, viscosity: 100 mPa·s, methoxy group content: 24 mass %

[0163] Alkoxysilane compound (a-3): "DOWSIL AY42-163" manufactured by Dow Corning Toray Co., Ltd., a trifunctional monomer raw material, viscosity: 30 mPa·s, methoxy content: 25 mass%

[0164] Alkoxysilane compound (a-4): "DOWSIL SR2402" manufactured by Dow Corning Toray Co., Ltd., a trifunctional monomer raw material, viscosity: 26 mPa·s, methoxy content: 31% by mass

[0165] Alkoxysilane compound (a-5): "X-40-9250" manufactured by Shin-Etsu Chemical Co., Ltd., difunctional monomer raw material and trifunctional monomer raw material, viscosity: 80 mPa·s, methoxy content: 25 mass%

[0166] Alkoxysilane compound (a-6): "KC-89S" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer raw material, viscosity: 5 mPa·s, methoxy group content: 45 mass %

[0167] Alkoxysilane compound (a-7): "X-40-9246" manufactured by Shin-Etsu Chemical Co., Ltd., difunctional monomer raw material and trifunctional monomer raw material, viscosity: 80 mPa·s, methoxy content: 12 mass%

[0168] Alkoxysilane compound (a-8): "Methyl silicate 51" manufactured by Colcoat Co., Ltd., tetrafunctional monomer raw material, viscosity: 5 mPa·s, methoxy content: 66 mass%

[0169] [Example 1: Preparation and Evaluation of Photocurable Organopolysiloxane]

[0170] 200 parts by mass of the alkoxysilane compound (a-1), 128 parts by mass of 2-hydroxyethyl acrylate, and sulfuric acid (50 ppm by mass) were placed in a reaction container, and the reaction was stirred for 8 hours at 70° C. while distilling off the generated methanol, thereby obtaining 294 g of a photocurable organopolysiloxane (A-1).

[0171] The obtained photocurable organopolysiloxane (A-1) was evaluated as follows.

[0172] (Content of polymerizable functional groups)

[0173] The obtained photocurable organopolysiloxane is subjected to 1The content of the polymerizable functional group was calculated from the intensity of the detected spectrum by H-nuclear magnetic resonance (NMR).

[0174] Specifically, in Example 1, 2-hydroxyethyl acrylate was used in the preparation of the photocurable organopolysiloxane, and the content of the polymerizable functional group bonded to the polysiloxane resin was calculated based on the peak intensity ratio of the peak (δ=3.97, CH2-O-Si) generated by the bonding of 2-hydroxyethyl acrylate and silicone oligomer via Si-OC bonds in the spectrum and the peak intensity ratio derived from the standard substance pre-added to the measurement sample.

[0175] In addition, the 1 H-NMR was carried out under the following conditions.

[0176] Measuring device: "AVANCE NEO400" manufactured by Bruker Japan Co., Ltd.

[0177] Magnetic field strength: 400MHz

[0178] Total times: 16 times

[0179] Solvent: Deuterated chloroform (CDCl3)

[0180] Sample concentration: 30mg / 0.6ml

[0181] (Residual amount of alkoxysilyl groups)

[0182] The obtained photocurable organopolysiloxane was subjected to the same conditions as those for the measurement of the content of the polymerizable functional group. 1 The alkoxysilyl group content was calculated from the detected spectrum intensity by H-NMR measurement.

[0183] Specifically, in Example 1, a silicone oligomer having a methoxy group was used in the preparation of the photocurable organopolysiloxane, and the residual amount of the alkoxysilyl group (methoxysilyl group) was calculated based on the peak intensity ratio of the methoxy group of the silicone oligomer in the spectrum (δ=3.52, Si-OCH3) and the peak intensity ratio derived from the standard substance pre-added to the measurement sample.

[0184] (Polysiloxane structure content)

[0185] The content of the polysiloxane structure in the photocurable organopolysiloxane was evaluated by ash measurement. Specifically, about 1.0 g of the obtained photocurable organopolysiloxane was weighed in a crucible and dried in a dryer at 130°C for 30 minutes. Thereafter, the crucible was moved to an electric furnace and calcined at 850°C for 3 hours. After cooling, the crucible was taken out, and the ash derived from the polysiloxane structure was calculated from the weight loss component, and evaluated according to the following criteria.

[0186] The greater the content of the polysiloxane structure, the higher the durability and weather resistance of the cured product.

[0187] (A): 45% by mass or more

[0188] (B): 35% by mass or more and less than 45% by mass

[0189] (C): less than 35% by mass

[0190] (Applicability Evaluation)

[0191] About 1.0 g of the obtained photocurable organopolysiloxane was weighed and the viscosity was measured using an E-type viscometer (Toki Sangyo, product name: TV-22) with a platform temperature set to 25°C, at a rotation speed of 100 rpm and a rotor No. 1, and evaluated according to the following criteria. The lower the viscosity, the better the coating properties.

[0192] (A): 100mPa·s or less

[0193] (B): More than 100 mPa·s and less than 150 mPa·s

[0194] (C): more than 150mPa·s

[0195] (Storage elastic coefficient evaluation)

[0196] 100 parts by mass of the obtained photocurable organopolysiloxane, 2 parts by mass of 1-hydroxycyclohexyl-phenyl ketone ("OMNIRAD 184" manufactured by IGM) as a photopolymerization initiator, and 0.02 parts by mass of p-methoxyphenol as a polymerization inhibitor were mixed, and diluted with propylene glycol monomethyl ether acetate as a solvent so that the solid content concentration became 50% by mass to prepare a photocurable composition.

[0197] The obtained photocurable composition was spin-coated on a 6-inch silicon wafer at 1500 rpm for 30 seconds, and then baked on a hot plate at 80°C for 60 seconds to form a coating film. At this time, the film thickness was about 2.0 μm. Then, an ultraviolet (UV) irradiation device (manufactured by Sanyong Electric Manufacturing Co., Ltd.) was used to irradiate the coating film with 100 mJ / cm2 , thereby obtaining a UV cured film.

[0198] The storage elastic coefficient E' of the obtained cured film at an indentation depth of 200 nm was measured using a nano indenter ("ENT2100" manufactured by Elionix) and evaluated according to the following criteria. The storage elastic coefficient E' is an indicator of the durability of the cured film, and a higher value is better.

[0199] (A): 1,500MPa or more

[0200] (B): 1,000 MPa or more and less than 1,500 MPa

[0201] (C): Less than 1,000MPa

[0202] (Reprocessability Evaluation)

[0203] The cured film produced in the storage elastic coefficient evaluation was immersed in sulfuric acid hydrogen peroxide (sulfuric acid:hydrogen peroxide water=4:1 (volume ratio)) for 5 minutes and then rinsed with ion exchange water for 30 seconds. The state of the cured film during the process was visually observed, and the reworkability of the cured film was evaluated according to the following criteria.

[0204] (A): The cured film was dissolved in sulfuric acid and hydrogen peroxide, and no residue remained on the silicon wafer.

[0205] (B): The cured film peeled off from the silicon wafer, and no residue remained on the silicon wafer.

[0206] (C): No change was found in the hardened film.

[0207] [Example 2 to Example 6 and Comparative Examples 1 and 2: Preparation and Evaluation of Photocurable Organopolysiloxane]

[0208] A photocurable organopolysiloxane was produced in the same manner as in Example 1 except that the alkoxysilane compound and 2-hydroxyethyl acrylate in the amounts shown in Table 1 were used, and the same evaluation as in Example 1 was performed. The results are shown in Tables 1 and 2.

[0209] [Table 1]

[0210]

[0211] [Table 2]

[0212]

[0213] In Comparative Example 6, a photocurable silicone monomer represented by the following formula was used instead of the photocurable organopolysiloxane.

[0214] [Chemistry 8]

[0215]

[0216] The results in Tables 1 and 2 show that a cured product having excellent durability and reworkability can be obtained by using an organopolysiloxane having a T unit ratio and the amounts of polymerizable functional groups and alkoxysilyl groups within specific ranges.

Claims

1. A photocurable organopolysiloxane having a polymerizable functional group represented by the following general formula (1) and an alkoxysilane group, wherein: The proportion of T units in the total siloxy units is 70 mol% or more, The photocurable organopolysiloxane contains 40% by mass or more of the polymerizable functional group represented by the general formula (1), and contains the alkoxysilyl group in a range of 0.1% by mass to 10% by mass. *—O—R 11 —Y (1) In the general formula (1), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, Y is a group containing a carbon-carbon unsaturated bond, * indicates the bonding position to the silicon atom of the organopolysiloxane.

2. The photocurable organopolysiloxane according to claim 1, wherein The polymerizable functional group represented by the general formula (1) is a polymerizable functional group represented by the following general formula (1-2), In the general formula (1-2), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, R 12 is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, * indicates the bonding position to the silicon atom of the organopolysiloxane.

3. The photocurable organopolysiloxane according to claim 1 or 2, wherein: The content of the polysiloxane structure is 35% by mass or more.

4. The photocurable organopolysiloxane according to claim 1 or 2, wherein: The viscosity at 25°C is 150 mPa·s or less. 5 . A photocurable organopolysiloxane composition comprising the photocurable organopolysiloxane according to claim 1 or 2 and a photopolymerization initiator. The photocurable organopolysiloxane composition according to claim 5 , which is a resist composition. 7 . A cured product, which is a cured product of the photocurable organopolysiloxane composition according to claim 5 .