Artificial board emulsifying wax as well as preparation method and application thereof
By introducing esterified modified nanoparticles and water-soluble polymer compounds into the emulsified wax, a stable interface film is formed, which solves the problems of large amount of emulsifier and poor stability, and realizes efficient and low-cost emulsified wax preparation, suitable for artificial Waterproof and moisture-proof application of the board.
Patent Information
- Application Number
- CN202310582180.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-22
Smart Images

Figure BDA0004242107270000121
Abstract
Description
Technical Field
[0001] The invention relates to an artificial board emulsified wax and a preparation method and application thereof, belonging to the technical field of chemical industry. Background Art
[0002] In most cases, the best form of paraffin wax is wax emulsion, i.e., emulsified wax, which has the advantages of no need for solvents, no need for heating, uniform film formation, high efficiency and convenience. Emulsified wax is used for coating, sizing, moisture-proofing, rust-proofing, and maintenance, which is a very important way to use special wax. Emulsified wax products are widely used in the processes of agriculture, papermaking, textiles, flooring, and automotive polishing. The main problems of emulsified wax in the prior art are few varieties, poor stability, small production scale, and failure to meet market needs.
[0003] In the 1970s, in the production of fiberboard and particleboard, most of the solid paraffin and molten paraffin were directly added to the board, but the effect was not good, mainly because the particles were large and the paraffin could not be evenly coated on the surface of the artificial board, resulting in reduced strength of the artificial board, easy cracking, and deformation, and reduced waterproof performance, greatly affecting product quality. Later, people began to use emulsified wax as a waterproof agent for artificial boards. Due to the small particle size of emulsified wax, in the process of preparing artificial boards, through effective demulsification, the wax particles can be precipitated and more evenly adsorbed on wood fibers or wood chips, which not only enhances the water resistance of artificial boards, but also reduces the consumption of paraffin.
[0004] CN104558634A discloses an emulsified paraffin for wood processing and a preparation method thereof. The emulsified paraffin is prepared from 30-60 parts by mass of paraffin, 6-15 parts by mass of a composite emulsifier and 25-55 parts by mass of water; the composite emulsifier is a mixture of a Span surfactant, a Tween surfactant, an alkylphenol polyoxyethylene ether and an alcohol. Although the emulsified paraffin has good stability, more emulsifiers are used, and the cost of the emulsified wax is high.
[0005] CN102766336A discloses a paraffin emulsion and a preparation method thereof. The main components and weight ratios of the paraffin emulsion are: 22-28 paraffin, 2-3 stearic acid and 2.2-2.8 ammonia water. Although the paraffin emulsion can reduce the amount of emulsifier, ammonia water needs to be added during the preparation process, and the emulsion is easily demulsified and precipitated when encountering acidic substances, which makes the stability of the paraffin emulsion worse.
[0006] CN101597482A discloses an emulsified paraffin waterproofing agent for medium density fiberboard. The emulsified paraffin waterproofing agent is prepared by emulsifying solid paraffin with sodium lauryl sulfate, Span-60, monoglyceride as emulsifiers, Peregal 0 (fatty alcohol polyoxyethylene ether), Tween-80 as catalysts, and polyvinyl alcohol as a colloid protective agent. The hydrophilic surfactants such as sodium lauryl sulfate used in the emulsified paraffin remaining in the fiberboard will have a serious impact on the waterproof performance of the fiberboard.
[0007] CN104004364A discloses a special environmentally friendly emulsified wax for artificial boards. The main components and contents of the emulsified wax are as follows: 42-75% of fully refined paraffin wax, 15-50% of microcrystalline wax, 35-55% of insect wax, 1-10% of palm wax, 18-33% of ozokerite, 8-17% of emulsifier, 7-14% of auxiliary emulsifier, and water balance. The special environmentally friendly emulsified wax for artificial boards has the characteristics of good miscibility, low melting point, strong adhesion, high water resistance, simple operation, convenient process, etc. It can improve the adhesion, water resistance, acid and alkali resistance of the wax film, and improve many shortcomings of paraffin emulsion. However, the emulsifier used in the emulsified wax is more, and the cost of the emulsified wax is higher.
[0008] CN101633785A discloses a paraffin emulsion and its preparation method and application. The paraffin emulsion comprises the following components in parts by weight: 8-20 parts of paraffin, 4-10 parts of hydrophilic nonionic surfactant, 8-20 parts of oil ester, and 50-80 parts of water. Among them, the hydrophilic nonionic surfactant includes fatty alcohol polyoxyethylene ether, and the oil ester includes stearic acid glyceryl. The shelf life of the paraffin emulsion is more than 12 months, but the amount of emulsifier used is huge, even exceeding the amount of paraffin.
[0009] The emulsified wax disclosed in the above prior art has one or more disadvantages such as large amount of emulsifier, high cost, poor water resistance, poor stability, etc. Therefore, it is urgent to provide an emulsified wax for artificial boards with low emulsifier amount, strong water resistance and strong stability. Summary of the invention
[0010] In order to solve the above technical problems, the purpose of the present invention is to provide an artificial board emulsified wax and its preparation method and application. The artificial board emulsified wax provided by the present invention has the advantages of less emulsifier usage, strong water resistance, good stability, etc.
[0011] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an artificial board emulsified wax, which comprises the following components based on its total mass of 100%: 20% to 40% paraffin wax, 0.5% to 2% esterified modified nanoparticles, 2% to 4% composite emulsifier, 0.2% to 1% water-soluble polymer compound and water balance (i.e., 53% to 77.3%); wherein the composite emulsifier comprises a mixture of glyceryl monostearate, Tween and fatty alcohol polyoxyethylene ether.
[0012] According to a specific embodiment of the present invention, preferably, based on the total mass of the artificial board emulsified wax as 100%, it includes the following components: 25% to 35% paraffin, 0.5% to 1% esterified modified nanoparticles, 2.5% to 3% composite emulsifier, 0.5% to 0.8% water-soluble polymer compounds and water balance (i.e., 60.2% to 71.5%).
[0013] In some specific embodiments of the present invention, the paraffin wax may include fully refined paraffin wax and / or semi-refined paraffin wax, etc., preferably semi-refined paraffin wax, specifically including No. 56 semi-refined paraffin wax, No. 58 semi-refined paraffin wax, etc.
[0014] In the above-mentioned artificial board emulsified wax, preferably, the esterified modified nanoparticles include esterified modified nano-SiO 2 And / or esterification modified nano Al 2 O 3 etc.; more preferably including esterified modified nano-SiO 2 .
[0015] In the above-mentioned artificial board emulsified wax, preferably, the esterified modified nanoparticles are octanol-modified nanoparticles. More preferably, the octanol-modified nanoparticles are prepared by the following steps: octanol and nanoparticles are reacted under the action of a catalyst, and the hydroxyl groups on the surface of the nanoparticles undergo an esterification reaction with octanol, so that the nanoparticles maintain their own hydrophilicity while increasing their lipophilicity, thereby obtaining octanol-modified nanoparticles. Wherein, the nanoparticles may include nano-SiO 2 and / or nano-Al 2 O 3 Preferably, the average particle size of the nanoparticles is 10 to 40 nm, more preferably 20 to 30 nm.
[0016] In some specific embodiments of the present invention, the octanol-modified nanoparticles can be prepared by conventional reflux method, microwave irradiation method, etc. The present invention does not specifically limit the specific preparation steps of the octanol-modified nanoparticles.
[0017] In some specific embodiments of the present invention, the catalyst used in the step of preparing the octanol-modified nanoparticles may be p-toluenesulfonic acid.
[0018] In some specific embodiments of the present invention, the mass ratio of octanol, nanoparticles, and catalyst in the preparation step of the octanol-modified nanoparticles can be (48-52):(20-30):(0.5-2), preferably 50:25:1.
[0019] The present invention creatively introduces esterification modified nanoparticles into the emulsified wax of artificial board, which at least plays the following roles. First, the surface of the esterification modified nanoparticles of the present invention has more hydroxyl groups and stronger hydrophilicity, and after esterification modification, the surface of the esterification modified nanoparticles has more lipophilic molecular chains, the lipophilic molecular chains of the nanoparticles in the dispersed phase emulsion are tightly entangled with the paraffin molecules, and the hydroxyl groups on the surface of the nanoparticles are in contact with the water phase, so the esterification modified nanoparticles have certain emulsification properties, and the amount of emulsifier can be greatly reduced when added to the emulsified wax. Moreover, compared with the amphiphilic nanoparticles surface-modified by silane coupling agents or saturated fatty acids, the esterification modified nanoparticles of the present invention have smaller steric hindrance and better dispersibility in the continuous phase. In the emulsification process, more esterification modified nanoparticles can be adsorbed around the paraffin particles, and the formed interface film is more solid, so that the emulsion stability is better. Secondly, the esterified modified nanoparticles of the present invention can be adsorbed at the oil / water interface, and are tightly adsorbed on the interface film between the two phases like a layer of "armor", and the strong rigid barrier generated by the solid particles at the interface is used to prevent and inhibit the aggregation and collision of paraffin wax, thereby improving the stability of the emulsified wax.
[0020] In the above-mentioned artificial board emulsified wax, preferably, the Tween in the composite emulsifier includes Tween 80.
[0021] In the above-mentioned artificial board emulsified wax, preferably, the fatty alcohol polyoxyethylene ether in the composite emulsifier includes AEO-9.
[0022] In the above-mentioned artificial board emulsified wax, preferably, the mixing mass ratio of glyceryl monostearate, Tween 80 and fatty alcohol polyoxyethylene ether AEO-9 in the composite emulsifier is (3.8-4.2):(2.8-3.2):(2.8-3.2), and more preferably is 4:3:3.
[0023] In the above-mentioned artificial board emulsified wax, preferably, the HLB value of the composite emulsifier is 9-10, and more preferably 10.
[0024] The composite emulsifier used in the present invention includes both lipophilic emulsifier and hydrophilic emulsifier, which can effectively reduce the interfacial tension between paraffin and water after interaction, and the obtained microemulsion has good film-forming effect and is not easy to demulsify.
[0025] In the above-mentioned artificial board emulsified wax, preferably, the water-soluble polymer compound includes one or a combination of sodium carboxymethyl cellulose, polyvinyl alcohol and polyvinyl pyrrolidone, etc.; more preferably, it includes sodium carboxymethyl cellulose.
[0026] The water-soluble polymer compound used in the present invention can reduce the Brownian motion of droplets, reduce the collision probability between droplets, and improve the chemical and mechanical stability of the emulsified wax. At the same time, it produces a synergistic effect with the esterified modified nanoparticles of the present invention to enhance the stability of the emulsion. In addition, the cations carried by the water-soluble polymer compound can cause the paraffin particles to repel each other in the interface film, further enhancing the stability of the emulsified wax.
[0027] In the above-mentioned artificial board emulsified wax, the water used can be deionized water.
[0028] According to a specific embodiment of the present invention, preferably, the average particle size of the droplets of the artificial board emulsified wax is 0.2-1.0 μm.
[0029] In the artificial board emulsified wax of the present invention, the esterified modified nanoparticles of the present invention produce a strong synergistic effect with the water-soluble polymer compound at the oil-water interface, the water-soluble polymer compound is adsorbed on the surface of the paraffin droplets, which is conducive to the formation of a stable interface film, and the molecular chains on the surface of the esterified modified nanoparticles and the molecular chains of the water-soluble polymer compound are entangled with each other, so that the mechanical strength and thickness of the oil-water interface film are further increased. At the same time, under the joint action of the composite emulsifier of the present invention, the mutual contact between the dispersed phases of the paraffin particles is blocked, and the stability of the emulsified wax is further enhanced.
[0030] The second aspect of the present invention provides a method for preparing the above-mentioned artificial board emulsified wax, which comprises the following steps:
[0031] (1) Based on the total mass of the artificial board emulsified wax as 100%, 20% to 40% (preferably 25% to 35%) of paraffin wax is heated and melted, 0.5% to 2% (preferably 0.5% to 1%) of esterified modified nanoparticles, 2% to 4% (preferably 2.5% to 3%) of composite emulsifier, and 0.2% to 1% (preferably 0.5% to 0.8%) of water-soluble polymer compound are added, and stirred uniformly to obtain an oil phase dispersed mixture;
[0032] (2) Under stirring conditions, 4% to 10% of hot water is added to the oil phase dispersed mixture, and stirred for a first time to form a W / O emulsion; then 10% to 20% of hot water is added, and stirred for a second time to form an O / D liquid crystal phase; and the remaining mass percentage of hot water is added, and stirred for a third time to form a stable O / W emulsion. After cooling, the artificial board emulsified wax is obtained.
[0033] In the above-mentioned preparation method, preferably, the temperature at which the paraffin is heated to melt in step (1) is 70 to 90°C.
[0034] In the above-mentioned preparation method, preferably, in step (1), the temperature at which the esterified modified nanoparticles, the composite emulsifier and the water-soluble polymer compound are added and stirred is 70 to 90°C.
[0035] In the above preparation method, preferably, the temperature of the hot water in step (2) is 70-90°C.
[0036] In the above preparation method, preferably, the first time in step (2) is 2 to 8 minutes.
[0037] In the above preparation method, preferably, the second time in step (2) is 10 to 20 minutes.
[0038] In the above preparation method, preferably, the third time in step (2) is 10 to 30 minutes.
[0039] In some specific embodiments of the present invention, the stirring speed in steps (1) and (2) can be conventionally adjusted by a person skilled in the art, and the present invention does not specifically limit it.
[0040] In some specific embodiments of the present invention, the cooling temperature in step (2) can be room temperature or below.
[0041] The third aspect of the present invention provides the use of the above-mentioned artificial board emulsified wax as a waterproofing agent in artificial boards.
[0042] In the above application, preferably, the artificial board includes one or a combination of particle board, fiber board and plywood.
[0043] In the above application, the amount of the artificial board emulsified wax added to the artificial board can be conventionally adjusted by those skilled in the art, and the present invention does not specifically limit it.
[0044] The present invention provides an artificial board emulsified wax and a preparation method and application thereof. The technical scheme of the present invention overcomes the shortcomings of the artificial board emulsified wax in the prior art, such as large amount of emulsifier, high cost, easy demulsification of the emulsified wax when encountering acid or alkali, poor waterproof performance, poor stability, etc. The present invention can greatly reduce the amount of emulsifier by introducing esterified modified nanoparticles, and the amount of emulsifier is only 2% to 4% of the total mass of the emulsified wax. At the same time, the synergistic effect between the esterified modified nanoparticles of the present invention and the water-soluble polymer compound further increases the mechanical strength and thickness of the oil-water interface film, and produces a strong synergistic effect with the composite emulsifier of the present invention, which can significantly enhance the stability of the emulsified wax. Therefore, the technical scheme of the present invention can greatly reduce the amount of emulsifier, reduce production costs, and ensure the stability of the emulsified wax. The artificial board emulsified wax of the present invention has good dispersibility, small droplet particle size, high stability, can be stored for a long time, and does not delaminate when standing for more than 8 months.
[0045] In summary, the preparation process of the artificial board emulsified wax of the present invention is simple, the operation and control are convenient, the production efficiency is high, the production cost is low, and the prepared emulsified wax has the advantages of good emulsification effect, acid resistance, alkali resistance, good waterproof performance, good stability, etc., and can be produced industrially on a large scale. The emulsified wax of the present invention is very suitable for use as a waterproofing agent in artificial boards, and can completely replace the solid paraffin used for artificial board processing to obtain waterproof and moisture-proof artificial boards with excellent dimensional stability, and has no adverse effects on the mechanical properties of artificial boards. DETAILED DESCRIPTION
[0046] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0047] The artificial board emulsified waxes provided in the following examples and comparative examples were evaluated and analyzed in the following manner.
[0048] 1. Centrifugal stability: The centrifugal stability of the emulsified wax was determined according to the method in GB11543-2008. The emulsified wax was centrifuged at 4000 r / min for 15 min and then observed to see if it was stratified.
[0049] 2. Static stability: Store the emulsified wax in a sealed container at room temperature for a period of time and observe whether it stratifies.
[0050] 3. Viscosity: According to the method in GB / T 1723-93, use a Tu-4 cup viscometer to test the viscosity of the emulsified wax.
[0051] 4. Average particle size: According to the method in ISO13321, a laser particle size analyzer is used to measure the droplet size distribution of the emulsified wax.
[0052] The raw material sources of the artificial board emulsified wax provided in the following embodiments and comparative examples include:
[0053] No. 56 semi-refined paraffin wax, PetroChina Daqing Refining and Chemical Company;
[0054] Nano-SiO 2 (average particle size is 20 nm), Hebei Zhuyan Alloy Materials Co., Ltd.;
[0055] Glyceryl monostearate, chemically pure, Xilong Scientific Co., Ltd.;
[0056] Fatty alcohol polyoxyethylene ether AEO-9, Tween 80, sodium carboxymethyl cellulose, octanol, ethanol, p-toluenesulfonic acid, analytical grade, Sinopharm Chemical Reagent Co., Ltd.
[0057] Example 1
[0058] This embodiment provides an artificial board emulsified wax, which includes the following components: 300g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 15g, composite emulsifier 30g, sodium carboxymethyl cellulose 8g, deionized water 647g.
[0059] The composite emulsifier is a mixture of glyceryl monostearate, Tween 80 and fatty alcohol polyoxyethylene ether AEO-9 in a mass ratio of 4:3:3, and the HLB of the composite emulsifier is 10.
[0060] Esterification modified nano-SiO 2 It is prepared by the following steps: octanol, nano-SiO 2 , p-toluenesulfonic acid in a mass ratio of 50:25:1 were placed in a reactor, the temperature was raised to 220°C, and constant temperature reflux was performed for 4 hours. After the reaction was completed, the product was centrifuged and washed 3 to 4 times with ethanol, and vacuum dried to obtain esterified modified nano-SiO 2 .
[0061] The preparation method of the artificial board emulsified wax provided in this embodiment comprises the following steps:
[0062] (1) Place 56# semi-refined paraffin in a reactor and heat to 80°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0063] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0064] Example 2
[0065] This embodiment provides an artificial board emulsified wax, which includes the following components: 400g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 20g, composite emulsifier 40g, sodium carboxymethyl cellulose 10g, deionized water 530g.
[0066] Among them, composite emulsifier and esterified modified nano-SiO 2 Same as in Example 1.
[0067] The preparation method of the artificial board emulsified wax provided in this embodiment comprises the following steps:
[0068] (1) Place 56# semi-refined paraffin in a reactor and heat to 70°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0069] (2) Deionized water was heated to 70°C, and then 53 g of 70°C hot water was added to the oil phase dispersed mixture under stirring conditions, and the mixture was stirred for 5 minutes to form a W / O emulsion; then 106 g of 70°C hot water was added, and the mixture was stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 70°C hot water was added, and the mixture was stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards was obtained.
[0070] Example 3
[0071] This embodiment provides an artificial board emulsified wax, which includes the following components: 250g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 10g, composite emulsifier 25g, sodium carboxymethyl cellulose 5g, deionized water 710g.
[0072] Among them, composite emulsifier and esterified modified nano-SiO 2 Same as in Example 1.
[0073] The preparation method of the artificial board emulsified wax provided in this embodiment comprises the following steps:
[0074] (1) Place 56# semi-refined paraffin in a reactor and heat to 90°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0075] (2) Deionized water is heated to 90° C., and then 70 g of 90° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 90° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 90° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0076] Example 4
[0077] This embodiment provides an artificial board emulsified wax, which includes the following components: 200g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 5g, composite emulsifier 20g, sodium carboxymethyl cellulose 2g, deionized water 773g.
[0078] Among them, composite emulsifier and esterified modified nano-SiO 2 Same as in Example 1.
[0079] The preparation method of the artificial board emulsified wax provided in this embodiment comprises the following steps:
[0080] (1) Place 56# semi-refined paraffin in a reactor and heat to 75°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0081] (2) Deionized water is heated to 75° C., and then 60 g of 75° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 120 g of 75° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 75° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0082] Example 5
[0083] This embodiment provides an artificial board emulsified wax, which includes the following components: 350g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 10g, composite emulsifier 35g, sodium carboxymethyl cellulose 8g, deionized water 597g.
[0084] Among them, composite emulsifier and esterified modified nano-SiO 2Same as in Example 1.
[0085] The preparation method of the artificial board emulsified wax provided in this embodiment comprises the following steps:
[0086] (1) Place 56# semi-refined paraffin in a reactor and heat to 85°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0087] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0088] Comparative Example 1
[0089] This comparative example provides an artificial board emulsified wax, which includes the following components: 300 g of No. 56 semi-refined paraffin, 90 g of a composite emulsifier, and 610 g of deionized water.
[0090] Wherein, the composite emulsifier is the same as that in Example 1.
[0091] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0092] (1) placing No. 56 semi-refined paraffin in a reaction kettle and heating it to 85° C. to melt, adding a composite emulsifier at this temperature and stirring evenly to obtain an oil phase dispersed mixture;
[0093] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0094] Comparative Example 2
[0095] This comparative example provides an artificial board emulsified wax, which includes the following components: 300 g of No. 56 semi-refined paraffin, 30 g of a composite emulsifier, and 670 g of deionized water.
[0096] Wherein, the composite emulsifier is the same as that in Example 1.
[0097] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0098] (1) placing No. 56 semi-refined paraffin in a reaction kettle and heating it to 80° C. to melt, adding a composite emulsifier at this temperature and stirring evenly to obtain an oil phase dispersed mixture;
[0099] (2) Deionized water is heated to 75° C., and then 40 g of 75° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 75° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 75° C. hot water is added, and stirred for 20 minutes to form an O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0100] Comparative Example 3
[0101] This comparative example provides an artificial board emulsified wax, which includes the following components: 300g of No. 56 semi-refined paraffin, 30g of a composite emulsifier, 8g of sodium carboxymethyl cellulose, and 662g of deionized water.
[0102] Wherein, the composite emulsifier is the same as that in Example 1.
[0103] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0104] (1) placing No. 56 semi-refined paraffin in a reaction kettle and heating it to 80° C. to melt, adding a composite emulsifier and sodium carboxymethyl cellulose at this temperature, and stirring evenly to obtain an oil phase dispersed mixture;
[0105] (2) Deionized water is heated to 75° C., and then 40 g of 75° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 75° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 75° C. hot water is added, and stirred for 20 minutes to form an O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0106] Comparative Example 4
[0107] This comparative example provides an artificial board emulsified wax, which includes the following components: 300g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 10g, composite emulsifier 30g, deionized water 660g.
[0108] Among them, composite emulsifier and esterified modified nano-SiO 2 Same as in Example 1.
[0109] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0110] (1) Place 56# semi-refined paraffin in a reactor and heat to 80°C to melt. At this temperature, add esterified modified nano-SiO 2 , a composite emulsifier, and stirring evenly to obtain an oil phase dispersed mixture;
[0111] (2) Deionized water is heated to 75° C., and then 40 g of 75° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 75° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 75° C. hot water is added, and stirred for 20 minutes to form an O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0112] Comparative Example 5
[0113] This comparative example provides an artificial board emulsified wax, which includes the following components: 300g of No. 56 semi-refined paraffin wax, amphiphilic nano-SiO 2 15g, composite emulsifier 30g, sodium carboxymethyl cellulose 8g, deionized water 647g.
[0114] Wherein, the composite emulsifier is the same as that in Example 1.
[0115] Amphiphilic Nano-SiO 2 It is prepared by the following steps: nano-SiO 2 The silane coupling agent KH-570 was placed in an appropriate amount of ethanol, ultrasonically dispersed for 5 minutes, and then stirred at 70°C for 6 hours. The product was centrifuged and dried to obtain amphiphilic nano-SiO 2 .
[0116] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0117] (1) Place 56# semi-refined paraffin in a reactor and heat to 80°C to melt. At this temperature, add amphiphilic nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0118] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0119] Comparative Example 6
[0120] This comparative example provides an artificial board emulsified wax, which includes the following components: 300g of No. 56 semi-refined paraffin wax, esterified modified nano-SiO 2 15g, composite emulsifier 30g, sodium carboxymethyl cellulose 8g, deionized water 647g.
[0121] The composite emulsifier is a mixture of glyceryl monostearate, Tween 80 and fatty alcohol polyoxyethylene ether AEO-9 in a mass ratio of 2:1:1, and the HLB value of the composite emulsifier is 8.5-9.0.
[0122] Esterification modified nano-SiO 2 Same as in Example 1.
[0123] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0124] (1) Place 56# semi-refined paraffin in a reactor and heat to 80°C to melt. At this temperature, add esterified modified nano-SiO 2 , composite emulsifier, sodium carboxymethyl cellulose, and stir evenly to obtain an oil phase dispersed mixture;
[0125] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0126] Comparative Example 7
[0127] This comparative example provides an artificial board emulsified wax, which includes the following components: 300 g of No. 56 semi-refined paraffin, 24 g of glyceryl monostearate, 12 g of fatty alcohol polyoxyethylene ether AEO-9, and 664 g of deionized water.
[0128] The preparation method of the artificial board emulsified wax provided in this comparative example comprises the following steps:
[0129] (1) placing No. 56 semi-refined paraffin in a reaction kettle and heating it to 80° C. to melt, adding glyceryl monostearate and fatty alcohol polyoxyethylene ether AEO-9 at this temperature, and stirring evenly to obtain an oil phase dispersed mixture;
[0130] (2) Deionized water is heated to 80° C., and then 40 g of 80° C. hot water is added to the oil phase dispersed mixture under stirring conditions, and stirred for 5 minutes to form a W / O emulsion; then 100 g of 80° C. hot water is added, and stirred for 15 minutes to form an O / D liquid crystal phase; the remaining 80° C. hot water is added, and stirred for 20 minutes to form a stable O / W emulsion. After cooling, an emulsified wax for artificial boards is obtained.
[0131] The evaluation and analysis results of the artificial board emulsified wax provided in the above Examples 1 to 5 and Comparative Examples 1 to 7 are shown in Table 1.
[0132] Table 1
[0133]
[0134] As can be seen from Table 1, under the premise that the same composite emulsifier is used as in Example 1, Comparative Example 1 uses a large amount of the composite emulsifier to prepare a milky white, delicate and uniform emulsified wax with the same appearance as Example 1, but the static stability of Comparative Example 1 can only reach 3 months. Comparative Examples 2 to 7 omit or replace one or several components in the emulsified wax of the present invention, and the appearance and stability of the emulsified wax prepared in these comparative examples are not good. The embodiments of the present invention can greatly reduce the amount of emulsifier by introducing esterified modified nanoparticles. At the same time, the synergistic effect between the esterified modified nanoparticles of the present invention and the water-soluble polymer compound further increases the mechanical strength and thickness of the oil-water interface film, and produces a strong synergistic effect with the composite emulsifier of the present invention. While significantly reducing the amount of emulsifier, the static stability of the emulsified wax is greatly improved, and there is no stratification after standing for more than 8 months.
[0135] The artificial board emulsified wax provided in the above-mentioned embodiments 1 to 5 and comparative examples 1 to 7 is used for fiberboard. The manufacturing method of the fiberboard is as follows: the pulped pre-treated wood with fiber dissociation is mixed with an adhesive and an emulsified wax to obtain a mixture, and the mixture is sequentially paved, pre-pressed and hot-pressed to obtain an artificial board. The amount of emulsified wax used in each cubic meter of artificial board material is 6 kg / m 3 The amount of urea-formaldehyde resin adhesive (Xinlai Plastic Synthetic Material Additive Factory) used is 80kg / m 3 The obtained artificial board was tested for waterproof performance, and the results are shown in Table 2. The waterproof performance of the artificial board was tested according to the method in GB / T 11718-2009 "Medium Density Fiberboard".
[0136] Table 2
[0137] Plate specifications 24h water absorption thickness expansion index / % Internal bonding strength index / MPa Example 1 18mmP2 6.1 1.42 Example 2 18mmP2 5.9 1.46 Example 3 18mmP2 6.0 1.47 Example 4 18mmP2 5.9 1.49 Example 5 18mmP2 6.0 1.50 Comparative Example 1 18mmP2 7.1 1.31 Comparative Example 2 18mmP2 9.5 1.20 Comparative Example 3 18mmP2 9.8 1.19 Comparative Example 4 18mmP2 7.0 1.35 Comparative Example 5 18mmP2 6.5 1.38 Comparative Example 6 18mmP2 9.2 1.15 Comparative Example 7 18mmP2 10 1.21
[0138] It can be seen from Table 2 that, from the performance of the artificial fiber board, the waterproof performance and internal bonding strength of the artificial board prepared by the emulsified wax of the embodiment of the present invention are better than the artificial board prepared by the emulsified wax lacking a certain component in the comparative example. The artificial board prepared by the emulsified wax provided by the present invention has excellent dimensional stability, good waterproof performance, and improved mechanical strength.
[0139] In summary, the preparation process of the artificial board emulsified wax of the present invention is simple, the operation and control are convenient, the production efficiency is high, the production cost is low, and the prepared emulsified wax has the advantages of small droplet size, small amount of emulsifier, good emulsification effect, good waterproof performance, good stability, etc., and can be industrially produced on a large scale. The emulsified wax of the present invention is very suitable for use as a waterproofing agent in artificial boards, and can completely replace the solid paraffin used for artificial board processing to obtain waterproof and moisture-proof artificial boards with excellent dimensional stability, and has no adverse effects on the mechanical properties of artificial boards.
[0140] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. An artificial board emulsified wax, based on the total mass of 100%, the artificial board emulsified wax comprises the following components: 20% to 40% paraffin wax, 0.5% to 2% esterified modified nanoparticles, 2% to 4% composite emulsifier, 0.2% to 1% water-soluble polymer compound and the balance water; wherein, The composite emulsifier comprises a mixture of glyceryl monostearate, Tween and fatty alcohol polyoxyethylene ether.
2. The artificial board emulsified wax according to claim 1, wherein Taking the total mass of the artificial board emulsified wax as 100%, The invention comprises the following components: 25% to 35% paraffin wax, 0.5% to 1% esterification modified nanometer particles, 2.5% to 3% composite emulsifier, 0.5% to 0.8% water-soluble high molecular compound and the balance of water.
3. The artificial board emulsified wax according to claim 1, wherein The esterified modified nanoparticles include esterified modified nano-SiO2 and / or esterified modified nano-Al2O3; preferably include esterified modified nano-SiO2.
4. The artificial board emulsified wax according to claim 3, wherein The esterification-modified nanoparticles are octanol-modified nanoparticles.
5. The artificial board emulsified wax according to claim 4, wherein The octanol-modified nanoparticles are prepared by the following steps: octanol and nanoparticles react under the action of a catalyst, and the hydroxyl groups on the surface of the nanoparticles react with octanol for esterification, so that the nanoparticles maintain their own hydrophilicity while increasing their lipophilicity, thereby obtaining octanol-modified nanoparticles.
6. The artificial board emulsified wax according to claim 5, wherein The mass ratio of octanol, nanoparticles and catalyst in the preparation step of the octanol-modified nanoparticles is (48-52):(20-30):(0.5-2), preferably 50:25:
1.
7. The artificial board emulsified wax according to claim 1, wherein The Tween in the composite emulsifier includes Tween 80; Preferably, the fatty alcohol polyoxyethylene ether in the composite emulsifier includes AEO-9.
8. The artificial board emulsified wax according to claim 7, wherein The mixing mass ratio of glyceryl monostearate, Tween 80 and fatty alcohol polyoxyethylene ether AEO-9 in the composite emulsifier is (3.8-4.2):(2.8-3.2):(2.8-3.2), preferably 4:3:
3.
9. The artificial board emulsified wax according to claim 8, wherein The HLB value of the composite emulsifier is 9-10.
10. The artificial board emulsified wax according to claim 1, wherein The water-soluble polymer compound includes one or a combination of sodium carboxymethyl cellulose, polyvinyl alcohol and polyvinyl pyrrolidone.
11. A method for preparing the artificial board emulsified wax according to any one of claims 1 to 10, comprising the following steps: (1) Based on the total mass of the artificial board emulsified wax being 100%, 20% to 40% of paraffin wax is heated and melted, 0.5% to 2% of esterified modified nanoparticles, 2% to 4% of a composite emulsifier, and 0.2% to 1% of a water-soluble polymer compound are added, and stirred uniformly to obtain an oil phase dispersed mixture; (2) Under stirring conditions, 4% to 10% of hot water is added to the oil phase dispersed mixture, and stirred for a first time to form a W / O emulsion; then 10% to 20% of hot water is added, and stirred for a second time to form an O / D liquid crystal phase; and the remaining mass percentage of hot water is added, and stirred for a third time to form a stable O / W emulsion. After cooling, the artificial board emulsified wax is obtained.
12. The preparation method according to claim 11, wherein In step (1), the temperature at which the paraffin is heated and melted is 70 to 90°C.
13. The preparation method according to claim 11, wherein: The temperature of the hot water in step (2) is 70-90°C.
14. The preparation method according to claim 11, wherein: The first time in step (2) is 2 to 8 minutes, the second time is 10 to 20 minutes, and the third time is 10 to 30 minutes.
15. Use of the artificial board emulsified wax according to any one of claims 1 to 10 as a waterproofing agent in artificial boards.
Citation Information
Patent Citations
Paraffin emulsion with ultrahigh solid content and preparation method thereof
CN102702755A
Emulsified paraffin for wood processing and preparation method thereof
CN104558634A
Defoamer containing high alcohol and preparation method thereof
CN107008035A
Modification of sand with superhydrophobic silica / wax nanoparticles
US10202548B1
Cited By
High-solid-content paraffin emulsion as well as preparation method and application thereof