Preparation method of healing type car cover protective film

By using raw materials such as aliphatic diisocyanate and hydroxy polyether polyol, combined with drying and winding calendering processes, a car protective film with self-healing ability is formed, solving the problems of low efficiency, high cost and short service life in the prior art. , realizes long-term protection and efficient self-repair of automobile paint.

CN118994664AInactive Publication Date: 2024-11-22NANTONG NAR MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311168260.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation methods for healing protective films are inefficient, cost-effective, poor repair effect, short service life, and difficult to meet the needs of widespread promotion.

Method used

Using raw materials such as aliphatic diisocyanate, hydroxy polyether polyol, catalyst, anti-UV additives, nanoparticles, etc., the drying, repair layer preparation and winding and calendering process is used to form a self-healing automotive protective film, and improve the curing coating. hydrophobicity and molecular chain migration and motility ability extend service life.

Benefits of technology

It realizes rapid self-healing and anti-yellowing of the automotive protective film, extends the service cycle, reduces the contamination of water and impurities, improves the self-repairing ability and production efficiency of the coating, and ensures long-term protection of the automotive paint surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention discloses a preparation method of a healing type vehicle cover protective film, and relates to the technical field of vehicle protective films, the preparation method comprises the following steps: S1, raw material preparation: aliphatic diisocyanate, hydroxyl polyether polyol, 20-30 parts of a catalyst, a chain extender, an anti-ultraviolet auxiliary agent, a solvent, inert silicone oil, nanoparticles, a dispersant and a defoaming agent; s2, drying treatment; s3, preparing a repairing layer; and S4, winding and calendering are conducted, specifically, the prepared protective film raw material is placed in a hopper, and an extruder heats and extrudes the automobile protective film raw material into a sheet-shaped structure. According to the preparation method, the disodium citrate solution is prepared, the nano particles are added into the disodium citrate solution, the nano particles can be effectively mixed with TPU pre-resin, so that the hydrophobicity of the surface of a cured coating is improved, polyurethane has more soft segment structures, the soft segment structures contain a large number of hydroxyl groups, migration movement of molecular chains can be achieved after film forming, and the hydrophobic property of the surface of the coating is improved. Rapid self-healing after the coating is damaged can be realized, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vehicle protective films, and in particular to a method for preparing a healing vehicle cover protective film. Background Art

[0002] At present, with cars, home furnishings and high-end equipment entering thousands of households and all walks of life, especially cars have become the basic equipment of most ordinary families. Cars are exposed to the external environment for a long time, and their original paint is easily damaged and needs frequent maintenance. How to protect the surfaces of cars, homes, etc. from extreme climate changes, especially the harsh external environment, has become a topic that must be considered in the industry, and it must also meet environmental protection requirements. Car protective film is a thermoplastic polyurethane film containing anti-UV polymers, anti-yellowing, super toughness, wear resistance, no yellowing, easy to stick, anti-collision and scratch resistance. After installation, the car paint surface can be isolated from the air, prevent acid rain, oxidation, scratches, and protect the paint surface for a long time. The following problems exist in the existing technology: 1. The existing preparation method of the healing car cover protective film cannot be processed in one go, resulting in large process cost waste and low efficiency, and cannot meet people's requirements; 2. The existing preparation method of the healing car cover protective film has an insufficient repair effect, is not convenient for long-term use, has a short service life, causes a high replacement cost for users, and is not convenient for widespread promotion and use. Summary of the invention

[0003] In order to solve the above technical problems, the technical solution adopted by the present invention is: A method for preparing a healing car cover protective film comprises the following steps: S1. Raw material preparation: aliphatic diisocyanate, hydroxy polyether polyol, 20-30 parts of catalyst, chain extender, anti-ultraviolet additive, solvent, inert silicone oil, nanoparticles, dispersant and defoamer; S2. Drying treatment: two TPU polyurethanes with different functions are put into drying respectively, the drying temperature is controlled at 65-75°C, the drying time is more than 5 hours, so that the moisture content of the raw materials is less than 100ppm; S3, preparation of repair layer: the raw materials for the preparation of the repair layer are 85 parts of aliphatic diisocyanate, 550 parts of hydroxy polyether polyol, 22 parts of catalyst, 30 parts of chain extender, 6 parts of anti-ultraviolet additive, 220 parts of solvent, 15 parts of inert silicone oil, 3 parts of nanoparticles, 6 parts of dispersant, and 6 parts of defoamer in a weight ratio; S4, winding and calendering: the prepared protective film raw material is placed in a hopper, and the extruder heats the automobile protective film raw material and extrude it into a sheet structure.

[0004] A further improvement of the technical solution of the present invention is that: S2 sends the above-mentioned two dried raw materials into two extruders respectively through a suction device, heats them to 175°C for dissolution, and extrude them separately after dissolution. After the raw materials are filtered, they are quickly sent to the same die head through a pump to generate a certain pressure for distribution and outflow molding, wherein the temperature of the filter, pipeline, and metering pump needs to be maintained between 185°C and 195°C.

[0005] The further improvement of the technical solution of the present invention is that: S3 aliphatic diisocyanate is selected from hexamethylene diisocyanate, hydroxy polyether polyol is selected from terminal hydroxyl polyether polyol and trihydroxy polyether polyol, the catalyst is a metal organic catalyst, including dibutyltin disilicate and bismuth neodecanoate, the anti-ultraviolet additive is selected from benzotriazole, the nanoparticles are nanoparticles modified with sodium citrate, nano-ferrosilicate, and nano-zinc oxide.

[0006] The further improvement of the technical solution of the present invention is: preparing a disodium citrate solution, adding nanoparticles to the disodium citrate solution, using a cell crusher to perform ultrasonic treatment on the mixed solution, using excess acetone to clean the ultrasonicated solution, and then putting the mixed solution into a vacuum drying oven for vacuum drying for 24 hours for standby use.

[0007] A further improvement of the technical solution of the present invention is that nitrogen is introduced into the reactor, aliphatic diisocyanate, hydroxy polyether polyol and solvent are added to the reactor, the temperature is lowered to 40-45°C, the remaining solvent is added to the reactor, and the prepared mixed liquid is applied by brushing, spraying, rolling or coating with a coater to form a self-healing coating after curing into a film.

[0008] A further improvement of the technical solution of the present invention is that: the S4 sheet-like structure of the automobile protective film is wound onto a calendering assembly, and the calendering assembly rolls the sheet-like structure of the automobile protective film into a thin film structure of the automobile protective film, and the thickness of the protective film is adjusted by adjusting the distance between the lower roller and the upper roller as needed.

[0009] Due to the adoption of the above technical solution, the present invention has the following technical advances compared with the prior art: The invention provides a preparation method of a healing car cover protective film. Under the joint action of nanoparticles and polyurethane, a disodium citrate solution is prepared, and the nanoparticles are added to the disodium citrate solution. The nanoparticles can be effectively mixed with the TPU pre-resin, thereby improving the hydrophobicity of the surface of the cured coating. The polyurethane has more soft segment structures, and the soft segment structure contains a large amount of hydroxyl groups. After film formation, the migration movement of molecular chains can be realized, and the coating can be quickly self-healed after being damaged, thereby improving the service life of the protective film.

[0010] The present invention provides a preparation method of a healing car cover protective film. Through the action of winding and calendering, a sheet-like car cover protective film is wound onto a calendering component, and the calendering component rolls the sheet-like car cover protective film into a thin film-like car cover protective film. The thickness of the protective film is adjusted by adjusting the distance between a lower roller and an upper roller as required. The distance between the lower roller and the upper roller is adjusted by a height adjustment device, and the car cover film with a thin film structure is rolled to a preset thickness, which is beneficial to process adjustment, so that the coating of the car cover protective film is more uniform, and the quality of the produced car cover protective film is uniform.

[0011] The present invention provides a preparation method of a healing car cover protective film. Through the joint action of an anti-ultraviolet additive, the anti-ultraviolet additive is selected from benzotriazole, which can effectively inhibit the yellowing tendency of polyurethane and extend the service life of the coating. At the same time, the surface of the TPU self-repairing coating has super hydrophobic properties, which can effectively reduce the contamination of water and impurities, thereby reducing the residence time of scratch impurities on the coating surface, thereby extending the self-repairing service life of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The overall process structure schematic diagram of a method for preparing a healing car cover protective film of the present invention; Figure 2 This is a schematic diagram of the process structure for preparing the repair layer of the present invention. Implementation

[0013] The present invention is further described in detail below in conjunction with embodiments: Example

[0014] like Figure 1-2 As shown, the present invention provides a method for preparing a healing car cover protective film, comprising the following steps: S1. Raw material preparation: aliphatic diisocyanate, hydroxy polyether polyol, 20-30 parts of catalyst, chain extender, anti-ultraviolet additive, solvent, inert silicone oil, nanoparticles, dispersant and defoamer; S2. Drying treatment: two TPU polyurethanes with different functions are put into drying respectively, the drying temperature is controlled at 65-75°C, the drying time is more than 5 hours, so that the moisture content of the raw materials is less than 100ppm; S3, preparation of repair layer: the raw materials for the preparation of the repair layer are 85 parts of aliphatic diisocyanate, 550 parts of hydroxy polyether polyol, 22 parts of catalyst, 30 parts of chain extender, 6 parts of anti-ultraviolet additive, 220 parts of solvent, 15 parts of inert silicone oil, 3 parts of nanoparticles, 6 parts of dispersant, and 6 parts of defoamer in a weight ratio; S4, winding and calendering: the prepared protective film raw material is placed in a hopper, and the extruder heats the automobile protective film raw material and extrude it into a sheet structure.

[0015] In this embodiment, a disodium citrate solution is prepared, and nanoparticles are added to the disodium citrate solution. The nanoparticles can be effectively mixed with the TPU pre-resin, thereby improving the hydrophobicity of the surface of the cured coating. The polyurethane has a relatively large number of soft segment structures, and the soft segment structure contains a large number of hydroxyl groups. After film formation, the molecular chain can migrate and the coating can quickly self-heal after damage, thereby increasing the service life of the protective film. The anti-ultraviolet additive is selected from benzotriazole, which can effectively inhibit the yellowing tendency of the polyurethane and extend the service life of the coating. At the same time, the surface of the TPU self-repairing coating has super-hydrophobic properties, which can effectively reduce the contamination of water and impurities, thereby reducing the residence time of scratch impurities on the coating surface, thereby extending the self-repairing service life of the coating. Example

[0016] like Figure 1-2 As shown, on the basis of Example 1, the present invention provides a technical solution: preferably, S2 respectively feeds the above-mentioned two dried raw materials into two extruders through a suction device, heats them to 175°C for dissolution, extrudes them respectively after dissolution, and then filters the raw materials and quickly feeds them into the same die head through a pump to generate a certain pressure for distribution and outflow molding, wherein the temperature of the filter, the pipeline, and the metering pump needs to be maintained between 185°C and 195°C, S3 aliphatic diisocyanate is selected from hexamethylene diisocyanate, hydroxyl polyether polyol is selected from terminal hydroxyl polyether polyol and trihydroxy polyether polyol, the catalyst is a metal organic catalyst, including dibutyltin disilicate and bismuth neodecanoate, the anti-ultraviolet additive is selected from benzotriazole, the nanoparticles are nanoparticles modified with sodium citrate, nano-ferric oxide, nano-zinc oxide, and lemon is configured Disodium citrate solution, add the nanoparticles to the disodium citrate solution, use a cell crusher to ultrasonically treat the mixed solution, use excess acetone to clean the ultrasonic solution, put the mixture into a vacuum drying oven, vacuum dry it for 24 hours, and set it aside. Nitrogen is introduced into the reactor, aliphatic diisocyanate, hydroxy polyether polyol and solvent are added to the reactor, the temperature is lowered to 40-45°C, the remaining solvent is added to the reactor, the prepared mixed solution is applied by brushing, spraying, rolling or coating with a coating machine, and a self-repairing coating is formed after solidification into a film. The S4 sheet-like structure of the automobile protective film is wound onto a calendering assembly, and the calendering assembly rolls the sheet-like structure of the automobile protective film into a thin film structure of the automobile protective film. The spacing between the lower roller and the upper roller is adjusted as needed to adjust the thickness of the protective film.

[0017] In this embodiment, the calendering component rolls the sheet-like structure of the automobile protective film into a thin film structure of the automobile protective film, and adjusts the distance between the lower roller and the upper roller as needed to adjust the thickness of the protective film. The height adjustment device is used to adjust the distance between the lower roller and the upper roller, and then the thin film structure of the car cover film is rolled to a preset thickness, which is beneficial to process adjustment, so that the coating of the automobile protective film is more uniform and the quality of the produced automobile protective film is uniform.

[0018] The working principle of the preparation method of the healing car cover protective film is described in detail below.

[0019] like Figure 1-2As shown, aliphatic diisocyanate, hydroxy polyether polyol, 20-30 parts of catalyst, chain extender, anti-ultraviolet additive, solvent, inert silicone oil, nanoparticles, dispersant and defoamer, two TPU polyurethanes with different functions are put into drying respectively, the drying temperature is controlled at 65-75°C, the drying time is more than 5 hours, so that the moisture content of the raw materials is less than 100ppm, the above two dried raw materials are respectively sent to two extruders through a suction device, heated to 175°C for dissolution, and extruded separately after dissolution. After filtering, the raw materials are quickly sent to the same die head through a pump to generate a certain pressure for distribution and outflow molding, wherein the temperature of the filter, pipeline and metering pump needs to be maintained between 185°C-195°C, and the raw materials for preparing the repair layer are 85 parts of aliphatic diisocyanate, 550 parts of hydroxy polyether polyol, 22 parts of catalyst, 30 parts of chain extender, 6 parts of anti-ultraviolet additive, and 220 parts of solvent by weight. 15 parts, inert silicone oil 15 parts, nanoparticles 3 parts, dispersant 6 parts, defoamer 6 parts, aliphatic diisocyanate selected from hexamethylene diisocyanate, hydroxy polyether polyol selected from terminal hydroxy polyether polyol and trihydroxy polyether polyol, catalyst is metal organic catalyst, including dibutyltin disilicate and bismuth neodecanoate, anti-ultraviolet additive is selected from benzotriazole, nanoparticles are nanoparticles modified by sodium citrate, nano ferrous oxide, nano zinc oxide, disodium citrate solution is prepared, nanoparticles are added to disodium citrate solution, cell crusher is used to ultrasonically treat the mixed solution at 8, after using excess acetone to clean the solution after ultrasonication, the mixture is easily put into a vacuum drying oven, vacuum dried for 24 hours, standby, nitrogen is introduced into the reactor, aliphatic diisocyanate, hydroxy polyether polyol and solvent are added to the reactor, the temperature is reduced to 40-45°C, the remaining solvent is added to the reactor, the prepared mixed solution,The coating is constructed by brushing, spraying, rolling or coating with a coating machine, and a self-repairing coating is formed after curing and film formation. The nanoparticles can be effectively mixed with the TPU pre-resin, thereby improving the hydrophobicity of the cured coating surface. Polyurethane has more soft segment structures, and the soft segment structure contains a large number of hydroxyl groups. After film formation, the molecular chain migration can be realized, and the coating can be quickly self-healed after damage, thereby increasing the service life of the protective film. The anti-ultraviolet additive is selected from benzotriazole, which can effectively inhibit the yellowing tendency of polyurethane and extend the service life of the coating. At the same time, the surface of the TPU self-repairing coating has super hydrophobic properties, which can effectively reduce the contamination of water and impurities, thereby reducing the residence time of scratch impurities on the coating surface, thereby extending the self-repairing service life of the coating. The raw materials of the car protective film are placed in the hopper, and the extruder heats and squeezes the raw materials of the car protective film into a sheet structure. The sheet structure of the car protective film is rolled to the calendering component, and the calendering component rolls the sheet structure of the car protective film into a thin film structure of the car protective film. The distance between the lower roller and the upper roller is adjusted as needed to adjust the thickness of the protective film. The calendering component rolls the sheet structure of the car protective film into a thin film structure of the car protective film. The distance between the lower roller and the upper roller is adjusted as needed to adjust the thickness of the protective film. The height adjustment device is used to adjust the distance between the lower roller and the upper roller, and then the thin film structure of the car cover film is rolled to a preset thickness, which is conducive to process adjustment, making the coating of the car protective film more uniform, and the quality of the produced car protective film is uniform. ,

[0020] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. A method for preparing a healing car cover protective film, comprising the following steps, characterized in that: S1. Raw material preparation: aliphatic diisocyanate, hydroxy polyether polyol, 20-30 parts of catalyst, chain extender, anti-ultraviolet additive, solvent, inert silicone oil, nanoparticles, dispersant and defoamer; S2. Drying treatment: two TPU polyurethanes with different functions are put into drying respectively, the drying temperature is controlled at 65-75°C, the drying time is more than 5 hours, so that the moisture content of the raw materials is less than 100ppm; S3, preparation of repair layer: the raw materials for the preparation of the repair layer are 85 parts of aliphatic diisocyanate, 550 parts of hydroxy polyether polyol, 22 parts of catalyst, 30 parts of chain extender, 6 parts of anti-ultraviolet additive, 220 parts of solvent, 15 parts of inert silicone oil, 3 parts of nanoparticles, 6 parts of dispersant, and 6 parts of defoamer in a weight ratio; S4, winding and calendering: the prepared protective film raw material is placed in a hopper, and the extruder heats the automobile protective film raw material and extrude it into a sheet structure.

2. The method for preparing a healing car cover protective film according to claim 1, characterized in that: S2 sends the above two dried raw materials into two extruders through a suction device, heats them to 175°C for dissolution, and extrude them separately after dissolution. The raw materials are filtered and then quickly sent into the same die head through a pump to generate a certain pressure for distribution and outflow molding. The temperature of the filter, pipeline and metering pump needs to be maintained between 185°C and 195°C.

3. The method for preparing a healing car cover protective film according to claim 1, characterized in that: S3 aliphatic diisocyanate is selected from hexamethylene diisocyanate, hydroxy polyether polyol is selected from terminal hydroxy polyether polyol and trihydroxy polyether polyol, the catalyst is a metal organic catalyst including dibutyltin disilicate and bismuth neodecanoate, the anti-ultraviolet additive is selected from benzotriazole, the nanoparticles are nanoparticles modified with sodium citrate, nano-ferrosilicate, and nano-zinc oxide.

4. The method for preparing a healing car cover protective film according to claim 3, characterized in that: Prepare a disodium citrate solution, add the nanoparticles to the disodium citrate solution, use a cell crusher to perform ultrasonic treatment on the mixed solution, use excess acetone to clean the ultrasonicated solution, and then put the mixed solution into a vacuum drying oven for vacuum drying for 24 hours for standby use.

5. The method for preparing a healing car cover protective film according to claim 4, characterized in that: Nitrogen is introduced into the reactor, and aliphatic diisocyanate, hydroxy polyether polyol and solvent are added into the reactor. The temperature is lowered to 40-45°C, and the remaining solvent is added into the reactor. The prepared mixed liquid is applied by brushing, spraying, rolling or coating with a coating machine, and a self-healing coating is formed after curing into a film.

6. The method for preparing a healing car cover protective film according to claim 1, characterized in that: The S4 sheet-like car protective film is wound to a calendering assembly, which rolls the sheet-like car protective film into a thin-film car protective film. The thickness of the protective film is adjusted by adjusting the distance between the lower roller and the upper roller as needed.