PEDOT: PSS flexible film based on phosphotungstic acid and preparation method thereof
By using phosphotungstic acid and gold nanoparticles for secondary doping in PEDOT:PSS materials, the stability and safety problems caused by doping modification in the prior art are solved, and high conductivity and environmentally friendly flexibility are achieved. Thin film materials, suitable for biomedical and flexible electronic fields.
Patent Information
- Application Number
- CN202410997784.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the doping modification method causes reduced solution stability, increased toxicity and environmental health problems for PEDOT:PSS materials and is not suitable for direct contact with organisms.
Phosphuttungstic acid and gold nanoparticles are used as new dopants to improve the conductivity and stability of PEDOT:PSS flexible films through secondary doping methods, ensuring environmental friendliness and operational safety, and the process is simple and suitable for large-scale industrial production.
It significantly improves the conductive properties and stability of PEDOT:PSS, avoids the toxicity and environmental pollution problems of traditional dopants, and achieves high conductivity and good mechanical stability of the material, which is suitable for biomedical and flexible electronic applications.
Smart Images

Figure CN118994682A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomaterials, in particular to a PEDOT:PSS flexible film based on phosphotungstic acid and a preparation method thereof. Background Art
[0002] PEDOT:PSS (poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid)), as a conductive polymer material, has been widely used in flexible electronics, optoelectronic devices and energy storage devices due to its excellent electrical conductivity, transparency, mechanical flexibility and chemical stability.
[0003] In the biomedical field, PEDOT:PSS is often used as an electrode material for brain-computer interfaces due to its excellent conductivity, flexibility, biocompatibility and low interface resistance. It collects and detects EEG signals and effectively stimulates nerves at low voltages to treat Parkinson's disease, epilepsy and other neurological diseases. In the optical field, due to the transparency of PEDOT:PSS, it can also be used in optical sensors and optical imaging equipment, playing an important role in bioimaging and optogenetics.
[0004] In order to further improve the performance of PEDOT:PSS, researchers have conducted various doping modification attempts, including doping with common dopants such as organic acids, inorganic acids, organic solvents and ionic liquids. Organic acid dopants such as formic acid, acetic acid and amino acids can improve the conductivity of PEDOT:PSS, but will lead to reduced solution stability and may introduce unpleasant odors or toxicity. Inorganic acid dopants such as sulfuric acid, phosphoric acid and hydrochloric acid can also improve conductivity, but may corrode equipment or cause harm to operators if not handled properly. Organic solvent dopants such as dimethyl sulfoxide (DMSO) and ethylene glycol (EG) can significantly improve the conductivity and smoothness of PEDOT:PSS films, but may cause environmental and health problems in applications. The films modified with ionic liquid dopants such as EMIM-TFSI (1-ethyl-3-methylimidazoline bis(trifluoromethylsulfonyl)imide) have high electrical properties, indicating that they have potential application prospects as transparent electrodes in flexible optoelectronic devices, but ionic liquids are usually more expensive and less stable than traditional organic solvents and salt dopants, which will limit their application in large-scale production. Although these conventional doping modification methods have made significant progress in improving the conductivity and other properties of PEDOT:PSS, they also have some shortcomings, such as reducing the stability of the solution, increasing toxicity and odor, and may even cause potential harm to the environment and operators, and are not suitable for direct contact with organisms. Summary of the invention
[0005] The purpose of the present invention is to solve the problems existing in the above-mentioned prior art and propose a method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid. 3 PW 12 O 40 ) and gold nanoparticles as new dopants, the PEDOT:PSS flexible film is modified by secondary doping. While improving the conductivity and stability of the PEDOT:PSS flexible film, it ensures environmental friendliness and operational safety. The process is simple and easy to large-scale industrial production.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid comprises the following steps:
[0008] Step S1, preparing a first mixed solution and a reduced phosphotungstic acid solution:
[0009] The phosphotungstic acid with a mass fraction of 4% to 6% and the PEDOT:PSS with a solid content of 1.0% to 1.3% are uniformly mixed to obtain a first mixed solution;
[0010] 2 mmol of phosphotungstic acid powder, 2 ml of 99% pure isopropanol, and 40 ml of deionized water were uniformly mixed, and then subjected to photocatalytic reduction reaction under ultraviolet light to obtain a reduced phosphotungstic acid solution;
[0011] Step S2, preparing the first mixed solution into a PEDOT:PSS film doped with phosphotungstic acid by a doctor blade method, and transferring the film onto a PET film after heating and curing to form a PEDOT:PSS flexible film with PET as a substrate;
[0012] Step S3, under ultraviolet light irradiation, immersing the PEDOT:PSS flexible film obtained in step S2 in a reduced phosphotungstic acid solution, adding an appropriate amount of tetrachloroauric acid solution according to the area of the film to be doped, so that the reduced phosphotungstic acid solution and the tetrachloroauric acid solution undergo a redox reaction to generate gold nanoparticles for secondary doping of the PEDOT:PSS flexible film, and after the doping is completed, the film is cleaned and dried to complete the preparation of the PEDOT:PSS flexible film based on phosphotungstic acid.
[0013] Furthermore, a UV lamp is used to generate ultraviolet light in both the process of preparing the reduced phosphotungstic acid solution and the secondary doping process.
[0014] Furthermore, the UV lamp irradiation time is 15-25 minutes.
[0015] Furthermore, the thickness of the PEDOT:PSS film doped with phosphotungstic acid prepared in step S2 is 40 μm to 50 μm after curing.
[0016] Furthermore, the drying condition in step S3 is at room temperature.
[0017] A PEDOT:PSS flexible film based on phosphotungstic acid is prepared by using phosphotungstic acid, gold nanoparticles and PEDOT:PSS composite liquid raw materials according to the preparation method of the PEDOT:PSS flexible film based on phosphotungstic acid.
[0018] After adopting the above technical solution, the present invention has the following advantages:
[0019] 1) The present invention significantly increases the conductivity of PEDOT:PSS by a secondary doping method of successively adding phosphotungstic acid and gold nanoparticles. In the first doping, the conductivity of PEDOT:PSS is increased by phosphotungstic acid doping. + The free carrier concentration on the chain, and the generation and uniform distribution of gold nanoparticles in the second doping based on this, further improve the electronic conductivity of the material, making the overall conductive performance significantly improved.
[0020] 2) The present invention uses phosphotungstic acid as the first doping agent, and phosphotungstic acid and PEDOT + The strong interaction between the chains improves the durability and stability of the film, so that the doped film exhibits good environmental stability and mechanical stability. Secondly, phosphotungstic acid has the advantages of low toxicity and good environmental compatibility, and does not produce volatile organic compound pollution, reducing the harm to the environment and operators. Compared with traditional organic acid and organic solvent dopants, the present invention is more environmentally friendly and safer.
[0021] 3) The present invention adopts the principle of generating gold nanoparticles by redox reaction of reduced phosphotungstic acid and tetrachloroauric acid. When a mask is used, the second doping process is controllable, patterned doping of gold nanoparticles can be achieved, and the generated gold nanoparticles can be evenly distributed on the surface and inside of the once-doped film, thereby ensuring the uniformity and excellent conductive properties of the film. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A flow chart of a method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid provided in an embodiment;
[0023] Figure 2 The following is a physical picture of a method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid, wherein (a) is a planar display picture, and (b) is a flexible display picture;
[0024] Figure 3Scanning electron microscope images of the thin film obtained by single doping (doping with phosphotungstic acid only) provided in the embodiment, wherein (a) is a 20 micron scanning electron microscope image, and (b) is a 500 nanometer scanning electron microscope image;
[0025] Figure 4 Scanning electron microscope images of thin films obtained by secondary doping provided in the embodiments, wherein (a) is a 20 micron scanning electron microscope image, and (b) is a 500 nanometer scanning electron microscope image;
[0026] Figure 5 The energy dispersion line spectrum results at 1 micron below the surface of the film obtained by secondary doping provided in the embodiment, wherein (a) is the surface scan result, and (b) is the relative content spectrum of the elements;
[0027] Figure 6 A graph showing the change of PEDOT:PSS flexible thin film resistor based on phosphotungstic acid with different phosphotungstic acid doping ratios provided in the embodiment;
[0028] Figure 7 The figure shows the change of resistance of the PEDOT:PSS flexible film based on phosphotungstic acid with the number of bending cycles at different bending degrees provided in the embodiment. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the accompanying drawings and implementation modes.
[0030] The present embodiment provides a PEDOT:PSS flexible film based on phosphotungstic acid, which is prepared by using phosphotungstic acid, gold nanoparticles and PEDOT:PSS composite liquid raw materials according to the following steps. Figure 1 As shown, including:
[0031] Step S1, preparing a first mixed solution and a reduced phosphotungstic acid solution:
[0032] Phosphotungstic acid with a mass fraction of 4% to 6% and PEDOT:PSS (1.0% to 1.3% solid content) are placed in a container and mixed evenly on a magnetic stirrer to obtain a first mixed solution.
[0033] 2mmol of phosphotungstic acid, 2ml of 99% pure isopropanol, and 40ml of deionized water were placed in a container and mixed evenly on a magnetic stirrer to obtain a second mixed solution. The second mixed liquid was placed under a 200W UV lamp for 20 minutes to fully react and obtain a reduced phosphotungstic acid solution.
[0034] Step S2: Preparation of PEDOT:PSS flexible film with PET as substrate
[0035] Step S2.1, draw 1.5 ml of the mixed liquid and drip it onto a 5×5 cm 2 The liquid was evenly coated on a glass sheet of the same specification using a scraper with a height of 1.65 mm. The liquid was cured on a hot plate at 90°C for 30 minutes to obtain a PEDOT:PSS film doped only with phosphotungstic acid on a glass substrate.
[0036] Step S2.2, after waiting for the film obtained in step S2.1 to cool down, the PEDOT:PSS thin film doped only with phosphotungstic acid on the glass substrate is immersed in deionized water for demolding and transferred to the PET film to obtain a PEDOT:PSS flexible film with PET as the substrate, which is then placed at room temperature to dry.
[0037] Step S3, immersing the PEDOT:PSS flexible film obtained in step S2 in a reduced phosphotungstic acid solution, dropping a tetrachloroauric acid solution and irradiating with a 200W UV lamp for 20 minutes; allowing the reduced phosphotungstic acid solution to undergo an oxidation-reduction reaction with the tetrachloroauric acid solution, then taking it out, rinsing it and drying it at room temperature to obtain a film as shown in FIG. Figure 2 The described phosphotungstic acid-based PEDOT:PSS flexible film.
[0038] The mechanism of the PEDOT:PSS flexible film based on phosphotungstic acid and its preparation method in this embodiment is:
[0039] Phosphotungstic acid has strong acidity and strong oxidizing properties and can react with PEDOT in PEDOT:PSS. + The chain reacts, making PEDOT + The positive charge on the chain increases. This charge transfer process increases the free carrier concentration in the PEDOT:PSS chain, thereby improving the conductivity of the material. After phosphotungstic acid doping, the anion PW in phosphotungstic acid 12 O 40 3- PSS - Competition with PEDOT + The positive charges on the chain produce an interaction, under which part of the PSS - is replaced or rearranged so that PEDOT + The distance between chains is reduced and the interchain interaction is enhanced, which promotes the efficient migration of charge carriers and improves the conductive properties of the material.
[0040] In the secondary doping process, the redox reaction is based on the following chemical reaction equation:
[0041]
[0042] Since both the reduced phosphotungstic acid solution and the PEDOT:PSS flexible film with PET as the substrate prepared in step 2 contain phosphotungstic acid, the gold nanoparticles generated by the redox reaction of phosphotungstic acid and tetrachloroauric acid are evenly distributed on the surface and inside of the PEDOT:PSS flexible film. These gold nanoparticles can further improve the conductivity of electrons, play a role in bridging the conductive chains, and enhance the overall conductivity. Through the above mechanism, phosphotungstic acid doping not only improves the conductive properties of PEDOT:PSS, but also enhances the stability and environmental friendliness of the material, avoiding the low biocompatibility, toxicity and volatility of traditional dopants.
[0043] Figure 3 The scanning electron microscope image of the film obtained by single doping (doping only with phosphotungstic acid) provided in the embodiment, wherein a is a 20 micron scanning electron microscope image, and b is a 500 nanometer scanning electron microscope image. Figure 3 a and Figure 3 As can be seen from b, the surface of the PEDOT:PSS film doped once (doped only with phosphotungstic acid) is smooth and uniform, and has better morphological characteristics.
[0044] Figure 4 The scanning electron microscope images of the thin film obtained by secondary doping provided in the embodiment, wherein (a) is a 20 micron scanning electron microscope image, and (b) is a 500 nanometer scanning electron microscope image. Figure 4 (a) and Figure 4 b It can be seen that the gold nanoparticles are evenly distributed on the PEDOT:PSS film doped with phosphotungstic acid and gold nanoparticles, and have excellent morphological characteristics.
[0045] Figure 5 The energy dispersion line spectrum results at 1 micron below the film surface obtained by secondary doping provided in the embodiment, wherein (a) is the surface scan result, and (b) is the element relative content spectrum. As can be seen from Figure (a), gold nanoparticles can be observed at 1 micron below the film surface, and as can be seen from Figure (b), the gold element content at 1 micron below the film surface reaches 20%wt. It can be seen that the gold nanoparticles are evenly distributed on the film surface and inside the film.
[0046] Figure 6 The graph of the PEDOT:PSS flexible thin film resistor based on phosphotungstic acid provided in the embodiment changes with different phosphotungstic acid doping ratios. Figure 6 It can be seen that the fixed area is 2×1.6cm 2 The conductivity of the film obtained at different phosphotungstic acid doping ratios is different. When the doping mass fraction is 4%-6% phosphotungstic acid, the conductivity of the obtained PEDOT:PSS film is optimal.
[0047] Figure 7The following is a graph showing the change in resistance of a PEDOT:PSS flexible film based on phosphotungstic acid with the number of bending cycles at different bending degrees provided in the embodiment. The graph shows the change in film resistance during 1000 bending cycles when the bending length of the film is 10%, 20%, 30% and 40% of the total length. Figure 7 It can be seen that under different bending degrees, the resistance change of the film in 1000 cycles is less than 5%. Therefore, it can be seen that the film has excellent flexibility, and after experiencing a large bending and multiple bending cycles, the film resistor can maintain a stable resistance value.
[0048] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application are within the scope of protection of the present invention.
Claims
1. A method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid, characterized in that: The following steps are involved: Step S1, preparing a first mixed solution and a reduced phosphotungstic acid solution: The phosphotungstic acid with a mass fraction of 4% to 6% and the PEDOT:PSS with a solid content of 1.0% to 1.3% are uniformly mixed to obtain a first mixed solution; 2 mmol of phosphotungstic acid powder, 2 ml of 99% pure isopropanol, and 40 ml of deionized water were uniformly mixed, and then subjected to photocatalytic reduction reaction under ultraviolet light to obtain a reduced phosphotungstic acid solution; Step S2, preparing the first mixed solution into a PEDOT:PSS film doped with phosphotungstic acid by a doctor blade method, and transferring the film onto a PET film after heating and curing to form a PEDOT:PSS flexible film with PET as a substrate; Step S3, under ultraviolet light irradiation, immersing the PEDOT:PSS flexible film obtained in step S2 in a reduced phosphotungstic acid solution, adding tetrachloroauric acid solution according to the area of the film to be doped, so that the reduced phosphotungstic acid solution and the tetrachloroauric acid solution undergo a redox reaction to generate gold nanoparticles for secondary doping of the PEDOT:PSS flexible film, and after the doping is completed, the film is cleaned and dried to complete the preparation of the PEDOT:PSS flexible film based on phosphotungstic acid.
2. The method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid according to claim 1, characterized in that: The process of preparing the reduced phosphotungstic acid solution and the secondary doping process both use a UV lamp to generate ultraviolet light.
3. The method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid according to claim 3, characterized in that: The UV lamp irradiation time is 15-25 minutes.
4. The method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid according to claim 1, characterized in that: The step S2 prepares a PEDOT:PSS film doped with phosphotungstic acid with a thickness of 40 μm to 50 μm after curing.
5. The method for preparing a PEDOT:PSS flexible film based on phosphotungstic acid according to claim 1, characterized in that: The drying condition in step S3 is at room temperature.