3D printing antibacterial correction material and preparation method thereof
The antibacterial correction materials containing MXene and zinc oxide were prepared through 3D printing technology, combined with the combination of ABS and polyurethane, and the problem of insufficient antibacteriality, intelligent monitoring and comfort of existing correction materials is solved, achieving efficient correction effects and personality Customization.
Patent Information
- Application Number
- CN202411076701.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing correction materials have shortcomings in antibacteriality, intelligent monitoring and comfort, and it is difficult to meet excellent performance at the same time, and it is difficult to achieve personalized customization.
Using 3D printing technology to prepare antibacterial correction materials containing MXene and in-situ synthetic zinc oxide. Through the composite of ABS plastic and polyurethane, combined with MXene-ZnO nanoparticles, the antibacterial, conductive and sensing functions of the material are realized, and the personality is achieved through 3D printing. Chemical design.
It improves the antibacterial and sensing properties of the correction materials, achieves long-lasting antibacterial effects and intelligent monitoring, improves the accuracy of correction and patient compliance, and improves the comfort and durability of the materials.
Smart Images

Figure CN118994725A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of 3D printing, and in particular relates to a 3D printing antibacterial correction material and a preparation method thereof. Background Art
[0002] In the fields of medical treatment and rehabilitation, corrective materials are widely used to correct and support human tissues, such as spinal braces, orthopedic correction, soft tissue correction, etc. At present, common corrective materials on the market include metal alloys, bioceramic materials and polymer materials. Metal alloys are widely used in corrective devices due to their high strength and durability, but they are rigid and lack flexibility, are not easy to be processed into complex shapes, and are prone to discomfort or even allergic reactions during long-term wear. Although ceramic materials have good aesthetics and biocompatibility, they are brittle and easy to break, which limits their application in corrective devices. Polymer materials are widely used because of their good flexibility and biocompatibility. However, traditional polymer corrective materials have antibacterial properties, lack of intelligence, comfort, and difficulty in achieving personalized customization, which limits their wide application.
[0003] Current antibacterial orthodontic materials are usually achieved by coating antibacterial agents on the surface of the materials, but this method has the problem that the antibacterial agents are easy to fall off and have poor durability. Therefore, introducing antibacterial materials into the correction materials themselves to maintain a stable antibacterial effect throughout the entire use cycle is a difficult problem that needs to be solved urgently. In addition, with the rapid development of intelligence, the intelligence of correction materials should also receive attention to realize intelligent monitoring (patient's wearing status, correction progress), etc., so as to make timely adjustments and interventions to formulate personalized treatment plans, improve treatment effects and patient compliance. In recent years, the development of 3D printing technology has also brought new opportunities for the preparation of correction materials. The application of 3D printing technology can achieve highly sophisticated and complex structural design, meet the personalized needs of different patients, and realize personalized customization.
[0004] Although some materials on the market have made breakthroughs in single performance, orthotic materials that can excel in all three aspects of antibacterial and intelligent monitoring are still scarce. Most orthotic materials cannot meet the requirements of antibacterial and intelligent monitoring at the same time, the antibacterial performance is difficult to sustain, and the intelligent monitoring function is single or ineffective. Therefore, exploring a corrective material with excellent antibacterial properties and intelligent monitoring and its preparation method will provide a new solution for the field of medical correction, significantly improving the treatment effect and patient experience. Summary of the invention
[0005] In order to solve the technical problems in the prior art that the existing corrective materials are insufficient in terms of comfort, antibacterial properties and intelligence in application, the present invention mainly provides a 3D printed antibacterial corrective material additive, a corrective material containing the additive and a preparation method of the corrective material. The specific scheme is as follows:
[0006] A 3D printed antibacterial orthotic additive comprising MXene and zinc oxide in situ synthesized on the surface of the MXene.
[0007] A correction material using the above-mentioned 3D printed antibacterial correction additive comprises, by weight, 0.1 to 5 parts of the additive according to claim 1, 70 to 100 parts of ABS plastic and 0.1 to 30 parts of polyurethane.
[0008] A method for preparing the above-mentioned correction material comprises the following steps:
[0009] a. ABS plastic and polyurethane are crushed to form fine powders respectively;
[0010] b. The crushed ABS plastic, polyurethane and additives are uniformly mixed using a ball mill to form a uniform composite powder;
[0011] c. Put the composite powder into a screw extruder, melt the composite powder and extrude the wire through heating and rotation of the screw;
[0012] d. stretching the extruded wire, rapidly cooling the stretched wire, shaping and stabilizing its size, and obtaining a corrective material wire; and printing the corrective material wire according to the model through a 3D printer to obtain the corrective material.
[0013] An application of the above-mentioned corrective additive in a device for correcting and / or supporting biological tissue, wherein when the stress on the article changes, the resistance of the article changes accordingly.
[0014] By adopting the above scheme, the method of the present invention has the following advantages:
[0015] 1. The present invention synthesizes ZnO nanoparticles on the surface of MXene. The ZnO nanoparticles are evenly distributed on the surface of MXene. The synthesized MXene-ZnO nanoparticles have antibacterial properties, electrical conductivity and sensing properties, and the performance is more stable when compounded with other components.
[0016] 2. The present invention enhances the antibacterial properties of the material, can effectively inhibit the growth of bacteria, and make the correction material have a lasting antibacterial effect, effectively prevent bacterial growth and infection, and reduce the risk of infection for patients.
[0017] 3. The correction material of the present invention has excellent sensing properties and can cooperate with the detection device to monitor parameters such as stress changes, timely understand the patient's wearing status and correction progress, and make timely adjustments and interventions to formulate appropriate treatment plans, such as replacing correction materials, to achieve intelligent correction, improve the accuracy and effectiveness of correction, and improve patient compliance.
[0018] 4. The present invention utilizes the flexibility of 3D printing technology to provide personalized solutions based on the patient's specific conditions and needs, realizes the integrated design and manufacturing of correction materials, simplifies the preparation process, reduces production costs, and improves production efficiency.
[0019] 5. The present invention adopts a composite of ABS and polyurethane to solve the problem of poor wearing comfort of traditional correction materials. The high strength of ABS and the flexibility of polyurethane ensure the stability and durability of the correction material during use. The flexibility of polyurethane improves the comfort of the correction material during wearing and enhances the compliance of patients.
[0020] 6. The present invention can improve the comfort of correction materials and ensure that appropriate correction force can be provided during the correction process, so as to improve the comfort of patients and reduce the discomfort and pain caused by excessive rigidity of the materials.
[0021] 7. The additives and correction materials of the present invention have a wide range of applications and can be used in correction insoles, spinal correction equipment and the like, and have a low threshold for use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The following are the XRD pattern (a), SEM photo (b), and TEM photo (c) of the additive of Example 1.
[0023] Figure 2 The tensile strength comparison graph (a), tensile modulus comparison graph (b), and elongation at break comparison graph (c) of ABS and the correction materials of Examples 1 to 3 and Comparative Example 1 are shown.
[0024] Figure 3 It is a comparison chart of OD values of the antibacterial properties of the correction materials of Examples 2, 4, 5, 6 and Comparative Example 2 (a), and a comparison chart of inhibition zones (b).
[0025] Figure 4 Comparison of the sensing performance of different MXene-ZnO contents (10N) of Examples 2, 4, 5, and 6 (a) and Example 2 under different stresses (b)
[0026] Figure 5 The corrective insole (a) and the spinal corrector (b) are obtained by 3D printing using the corrective material of Example 2. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Embodiment 1:
[0029] (1) Preparation of MXene-ZnO additive: Weigh a certain amount of MXene powder and disperse it in an appropriate amount of deionized water by ultrasonication, add 0.05 mol / L zinc acetate dihydrate, and stir mechanically for 30 min; prepare 2 mol / L sodium hydroxide solution, slowly add it dropwise to the above solution while stirring, and adjust the pH to 11; then pour the mixed solution into the polytetrafluoroethylene liner of the reactor, put the reactor into an oven for hydrothermal reaction to synthesize ZnO powder in situ on the MXene surface; after the reaction is completed, wait for the reactor to cool, filter to obtain MXene-ZnO nanocomposite powder, first wash with deionized water to neutrality, then wash with anhydrous ethanol for 3 times, and freeze-dry for 24 h to obtain the additive.
[0030] The XRD spectrum of the obtained sample is as follows Figure 1 As shown in (a), there are characteristic diffraction peaks of ZnO at 31.8°, 34.4°, 36.2°, 47.6°, 56.6°, 62.9°, 66.4° and 67.9°, indicating that high-purity ZnO is generated in the sample. Figure 1 (b) SEM and Figure 1 The TEM image in (c) shows that nano-ZnO is evenly distributed on the MXene surface, indicating that ZnO nanoparticles are evenly distributed on the MXene surface and MXene-ZnO nanoparticles are successfully synthesized.
[0031] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles are crushed into fine powders by freeze-crushing or shear milling; 90 parts by mass of the crushed ABS powder, 8 parts by mass of polyurethane powder, and 2 parts by mass of MXene-ZnO additives are weighed and mixed evenly in a ball mill at a speed of 1000 r / min for 2 h to form a uniform composite powder; the mixed composite powder is placed in a screw extruder, and the temperature of the screw extruder is set (the temperature of the first heating zone is 200°C, the temperature of the second heating zone is 220°C, the temperature of the third heating zone is 240°C, and the nozzle temperature is 230°C). The composite powder is melted and extruded into wires by heating and rotating the screw; the extruded wires are stretched, and the stretched wires are quickly cooled by a water bath or air cooling system to shape and stabilize their size to obtain the final corrected wires.
[0032] (3) Preparation of correction materials based on 3D printing: Load the filament into the feed port of the 3D printer, set the working parameters of the 3D printer, and print through the imported STL model. The printing parameters are: nozzle temperature of 250°C, nozzle diameter of 0.4 mm, printing speed of 40 mm / min, and thickness of 0.25 mm.
[0033] Embodiment 2:
[0034] The difference from Example 1 is:
[0035] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles were crushed into fine powders by freeze-crushing or shear milling. 80 parts of crushed ABS powder, 18 parts of polyurethane powder, and 2 parts of MXene-ZnO additive were weighed and mixed evenly in a ball mill. The speed was set to 1000 r / min and the mixing time was 2 h to form a uniform composite powder.
[0036] Embodiment 3:
[0037] The difference from Example 1 is:
[0038] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles were crushed into fine powders by freeze-crushing or shear milling. 70 parts of crushed ABS powder, 28 parts of polyurethane powder, and 2 parts of MXene-ZnO additive were weighed and mixed evenly in a ball mill. The speed was set to 1000 r / min and the mixing time was 2 h to form a uniform composite powder.
[0039] Embodiment 4:
[0040] The difference from Example 1 is:
[0041] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles were crushed into fine powders by freeze-crushing or shear milling. 80 parts by mass of the crushed ABS powder, 19 parts by mass of polyurethane powder, and 1 part by mass of MXene-ZnO additive were weighed and mixed evenly in a ball mill. The speed was set to 1000 r / min and the mixing time was 2 h to form a uniform composite powder.
[0042] Embodiment 5:
[0043] The difference from Example 1 is:
[0044] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles were crushed into fine powders by freeze-crushing or shear milling. 80 parts by mass of the crushed ABS powder, 17 parts by mass of polyurethane powder, and 3 parts by mass of MXene-ZnO additive were weighed and mixed evenly in a ball mill. The speed was set to 1000 r / min and the mixing time was 2 h to form a uniform composite powder.
[0045] Embodiment 6:
[0046] The difference from Example 1 is:
[0047] (2) Preparation of ABS / PU / MXene-ZnO composite wires: ABS plastic and polyurethane particles were crushed into fine powders by freeze-crushing or shear milling. 80 parts of crushed ABS powder, 15 parts of polyurethane powder, and 5 parts of MXene-ZnO additive were weighed and mixed evenly in a ball mill. The speed was set to 1000 r / min and the mixing time was 2 h to form a uniform composite powder.
[0048] Comparative Example 1:
[0049] (1) Preparation of ABS wire: ABS plastic is subjected to freeze-crushing or shear milling; 100 parts by mass of the crushed ABS powder are weighed and uniformly mixed in a ball mill, and the speed is set to 1000 r / min for 2 h to form a uniform composite powder; the ABS powder is put into a screw extruder, and the temperature of the screw extruder is set (the temperature of the first heating zone is 200°C, the temperature of the second heating zone is 220°C, the temperature of the third heating zone is 240°C, and the nozzle temperature is 230°C), and the composite powder is melted and extruded into wire through heating and screw rotation; the extruded wire is stretched, and the stretched wire is quickly cooled by a water bath or air cooling system to shape and stabilize its size to obtain the final corrected wire.
[0050] (3) Preparation of correction materials based on 3D printing: Load the filament into the feed port of the 3D printer, set the working parameters of the 3D printer, and print through the imported STL model. The printing parameters are: nozzle temperature of 250°C, nozzle diameter of 0.4 mm, printing speed of 40 mm / min, and thickness of 0.25 mm.
[0051] Comparative Example 2:
[0052] (1) Preparation of ABS / PU composite wire: ABS plastic and polyurethane particles are crushed into fine powder by freezing or shearing milling; 80 parts by mass of the crushed ABS powder and 20 parts by mass of the polyurethane powder are weighed and mixed evenly in a ball mill, and the speed is set to 1000 r / min for 2 h to form a uniform composite powder; the mixed composite powder is placed in a screw extruder, and the temperature of the screw extruder is set (the temperature of the first heating zone is 200°C, the temperature of the second heating zone is 220°C, the temperature of the third heating zone is 240°C, and the nozzle temperature is 230°C), and the composite powder is melted and extruded into wire by heating and rotating the screw; the extruded wire is stretched, and the stretched wire is quickly cooled by a water bath or air cooling system to shape and stabilize its size to obtain the final corrected wire.
[0053] (2) Preparation of correction materials based on 3D printing: Load the filament into the feed port of the 3D printer, set the working parameters of the 3D printer, and print through the imported STL model. The printing parameters are: nozzle temperature of 250°C, nozzle diameter of 0.4 mm, printing speed of 40 mm / min, and thickness of 0.25 mm.
[0054] Example sample test:
[0055] The mechanical properties of the correction material were measured using an electronic universal tensile testing machine. The mechanical strength and elongation at break of the correction wire prepared in Test Examples 1, 2, and 3 were compared with those in Comparative Example 1. The results are as follows: Figure 2 As shown in (a)(b)(c), the mechanical strength of the wire material decreases with the addition of PU, while the elongation at break increases significantly, indicating that the addition of PU improves the flexibility of the correction material.
[0056] The OD value (600nm) and the diameter of the inhibition zone were used to characterize the antibacterial properties of the samples. The correction materials of Examples 2, 4, 5, 6 and Comparative Example 2 were 3D printed into samples of the same size, and Escherichia coli and Staphylococcus aureus were selected for testing. The results are shown in Figure 2. Figure 3 As shown in the figure, the incorporation of MXene-ZnO additives significantly improved the antibacterial properties of the corrective material, and the antibacterial rate gradually increased with the addition of MXene-ZnO additives.
[0057] A digital multimeter was used to measure the sensing performance of the correction material and evaluate its intelligent monitoring capability. The correction materials of Examples 2, 4, 5, 6 and Comparative Example 2 were 3D printed into samples of the same size, placed in a stress-free state, the initial resistance value was recorded, stress was gradually applied, the corresponding resistance change was recorded, and the sensing sensitivity was calculated. The results are shown in Figure 2. Figure 4As shown in a, by comparison, the incorporation of MXene-ZnO additives gives the correction material sensing properties, and the sensing properties increase with the increase in the content of MXene-ZnO additives. It can be seen that the correction material of the present invention has high sensitivity and can accurately monitor subtle stress changes, thereby judging the patient's movements and identifying the patient's correction status.
[0058] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present invention.
Claims
1. A 3D printed antibacterial corrective additive, characterized in that: It includes MXene and zinc oxide synthesized in situ on the surface of MXene.
2. The 3D printed antibacterial corrective additive according to claim 1, characterized in that: Its preparation comprises the following steps: S1, take MXene powder and disperse it in water by ultrasonication, add zinc acetate, and mix well; S2, preparing a sodium hydroxide solution, slowly adding it dropwise into the reaction system while stirring, adjusting the pH of the system to 10.5-11.5, and performing a hydrothermal reaction; S3, after the reaction is completed, cool to room temperature, separate the precipitate, wash the precipitate with water until it is neutral, then wash it thoroughly with ethanol, and freeze-dry it to obtain the product.
3. The 3D printed antibacterial correction additive according to claim 2, characterized in that: The molar ratio of the MXene powder to zinc acetate in S1 is (2-3):1; the concentration of zinc acetate is 0.01-0.1 mol / L; and the concentration of sodium hydroxide is 1-2 mol / L.
4. The 3D printed antibacterial corrective additive according to claim 2, characterized in that: The temperature of the hydrothermal reaction in S2 is 100-120°C, and the reaction time is 20-28h.
5. A correction material using the 3D printed antibacterial correction additive according to any one of claims 1 to 4, characterized in that: Calculated by weight, it comprises 0.1 to 5 parts of the additive according to claim 1, 70 to 100 parts of ABS plastic and 0.1 to 30 parts of polyurethane.
6. A method for preparing the correction material according to claim 5, characterized in that: The following steps are involved: a. ABS plastic and polyurethane are crushed to form fine powders respectively; b. The crushed ABS plastic, polyurethane and additives are uniformly mixed using a ball mill to form a uniform composite powder; c. Put the composite powder into a screw extruder, melt the composite powder and extrude the wire through heating and rotation of the screw; d. stretching the extruded wire, rapidly cooling the stretched wire, shaping and stabilizing its size, and obtaining a corrective material wire; and printing the corrective material wire according to the model through a 3D printer to obtain the corrective material.
7. The method for preparing a correction material according to claim 6, characterized in that: The ball milling speed in step b is 800-1500 r / min, and the time is 2-4 h.
8. The method for preparing a correction material according to claim 6, characterized in that: In step c, the temperature of the screw extruder is set as follows: the temperature of the first heating zone is 180-200°C, the temperature of the second heating zone is 200-220°C, the temperature of the third heating zone is 220-240°C, and the nozzle temperature is 210-230°C.
9. The method for preparing a correction material according to claim 6, characterized in that: In step d, the 3D printing temperature is 250° C., the nozzle diameter is 0.2-0.5 mm, the printing speed is 30-60 mm / min, and the layer thickness is 0.1-0.4 mm.
10. Use of the corrective additive according to claim 1 in preparing an article for correcting and / or supporting biological tissue, characterized in that: When the stress on the object changes, the resistance of the object changes accordingly.
Citation Information
Patent Citations
3D printing material having self-cleaning antibacterial function as well as preparation method and application of 3D printing material
CN104530668A
ABS material with antibacterial function used for 3D printing and preparation method of ABS material
CN107418130A
Three-dimensional printed MXene composite scaffold as well as preparation method and application thereof
CN113262081A
MXene-zinc oxide nano composite material, preparation method thereof and recyclable hydrophobic antibacterial material prepared from MXene-zinc oxide nano composite material
CN114747593A
Face warm-keeping protection tool in low-temperature environment
CN116674261A