Long-life damping rubber material as well as preparation method and application thereof

By using natural rubber, itaconic acid rubber and Eucommia rubber in rubber materials, and introducing a three-dimensional hybrid stacking system of graphene and carbon nanotubes, the problem of insufficient tear strength and fatigue performance of rubber bushings is solved, and the further development is achieved. High tear strength and fatigue life extend the service life.

CN118994830APending Publication Date: 2024-11-22DONGFENG COMML VEHICLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411152245.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During long-term use, existing rubber bushings are prone to decrease tear strength due to external forces and environmental factors, and insufficient fatigue performance, resulting in short service life.

Method used

A raw rubber material consisting of natural rubber, itaconic acid rubber and eucommia rubber is used, and graphene and carbon nanotubes are introduced as thermal conductors to form a three-dimensional hybrid stacking system through dopamine modification to enhance the thermal conductivity and machinery of the rubber material. Performance, preventing crack propagation and media diffusion.

Benefits of technology

It significantly improves the tear strength and fatigue life of rubber materials, extends service life, and improves damping and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003966220000031
    Figure BDA0005003966220000031
  • Figure BDA0005003966220000071
    Figure BDA0005003966220000071
  • Figure BDA0005003966220000151
    Figure BDA0005003966220000151
Patent Text Reader

Abstract

The invention belongs to the field of rubber materials, and relates to a long-life damping rubber material as well as a preparation method and application thereof. Raw rubber in the long-life vibration reduction rubber material is composed of natural rubber, itaconate rubber and eucommia ulmoides rubber, and a heat conduction agent is composed of graphene and carbon nanotubes. At normal temperature, the eucommia ulmoides rubber exists in a matrix in a nanocrystal form, so that initiation and expansion of cracks can be hindered, and the tearing strength of the rubber material is improved; medium diffusion can be hindered, and aging of the rubber material is inhibited; in the nanocrystal melting process, a large amount of heat can be absorbed, and the destructive effect of temperature rise on the molecular structure of the rubber material is reduced; the itaconate rubber can improve the vibration damping performance of the rubber material; the graphene and the carbon nanotubes can synergistically improve the mechanical properties and heat conduction and heat dissipation properties of the rubber matrix. Therefore, the tear strength of the rubber material prepared by the invention is high and can be 45.3 kN / m, and the tensile fatigue life is long and can reach 29,000-35,000 times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rubber materials, and in particular relates to a long-life vibration-damping rubber material and a preparation method and application thereof. Background Art

[0002] Rubber bushings are accessories used on the outside of mechanical parts to seal and protect against wear. They refer to annular sleeves that act as gaskets. As an important vibration-damping component of the automobile chassis, rubber bushings play an important role in the comfort and stability of the entire vehicle. They can effectively absorb and isolate vibrations from the road and the engine. However, in the actual development process, the durability of rubber bushings often becomes a key factor restricting the performance of the entire vehicle. Studies have shown that during the driving process of a car, rubber bushings will be continuously stretched and compressed by external forces, and will also be affected by external heat, ozone, etc., resulting in the breaking of chemical bonds on the molecular chain, resulting in a decrease in the performance of the rubber material. When the local deformation stress borne by the rubber bushing exceeds the elongation or stress limit of the rubber material, failure occurs.

[0003] Traditional rubber bushings for heavy truck chassis are made of natural rubber, which is mainly polyisoprene and contains a small amount of protein, water, resin acid, sugar and inorganic salt. Although it has high elasticity, high tensile strength and excellent tear resistance, it has poor oxygen and ozone resistance, is prone to aging and deterioration, has low acid and alkali corrosion resistance and low heat resistance. In addition, natural rubber has poor damping and vibration reduction performance because its molecular chain lacks large steric hindrance groups.

[0004] Eucommia rubber is an isomer of natural rubber, and its main component is trans-polyisoprene. Compared with natural rubber, eucommia rubber has the advantages of good dynamic fatigue resistance and low heat generation. Studies have shown that when eucommia rubber and natural rubber are co-vulcanized, eucommia rubber is distributed in the natural rubber in the form of sheets, which will cause the rubber material to tear along the surface of the lamellar structure, and the tear strength will drop by up to 20%, which will lead to a decrease in the fatigue performance of the rubber material. Chinese patent document CN111454493A (publication date: July 28, 2020) uses raw rubber of natural rubber, eucommia rubber, isoprene rubber, and butadiene rubber to prepare ball joints for air suspension. By controlling the content of eucommia rubber within a certain range, the tear strength decrease rate of the ball joint can be reduced and the fatigue performance of the ball joint can be improved, but the tear strength and fatigue performance of the ball joint still have a lot of room for improvement. Summary of the invention

[0005] The invention provides a long-life vibration-damping rubber material and a preparation method and application thereof, aiming to improve the tear strength and fatigue performance of the rubber material to extend its service life.

[0006] In order to achieve the above invention purpose, the raw rubber of the present invention is composed of natural rubber, itaconate rubber and eucommia rubber. At room temperature, eucommia rubber exists in the matrix in the form of nanocrystals, which can hinder the initiation and expansion of cracks, thereby avoiding the decrease of the tear strength of the rubber material. At the same time, eucommia rubber can hinder the diffusion of the medium and inhibit the aging of the rubber; eucommia rubber nanocrystals are easy to absorb heat and melt, which can reduce the destructive effect of temperature increase on the matrix; the ester group contained in itaconate rubber can form a hydrogen bond network with various additives inside the rubber material, limit the movement of the molecular chain inside the rubber material, increase the internal friction of the rubber material, and thus increase the damping performance of the rubber material. The present invention also introduces a thermal conductor composed of graphene and carbon nanotubes into the rubber material. The one-dimensional graphene and the two-dimensional carbon nanotubes are modified by dopamine to form a three-dimensional hybrid stacking system, which has a synergistic enhancement effect on the rubber matrix, and the thermal conductivity of the three-dimensional hybrid stacking system is improved. Graphene can improve the heat dissipation of the rubber material. Therefore, the heat generated by the rubber material can be quickly conducted out, thereby slowing down the aging process of the rubber material and extending the service life of the rubber material.

[0007] Based on this, the present invention provides the following technical solutions:

[0008] A first aspect of the present invention provides a long-life vibration-damping rubber material, wherein the long-life vibration-damping rubber material is kneaded by rubber raw materials, and the rubber raw materials, measured by weight percentage, include:

[0009]

[0010]

[0011] The raw rubber consists of natural rubber, itaconate rubber and eucommia rubber, wherein the eucommia rubber accounts for 10wt% to 25wt% of the total raw rubber, the itaconate rubber accounts for 30wt% to 70wt% of the total raw rubber, and the natural rubber accounts for 20wt% to 45wt% of the total raw rubber.

[0012] In any embodiment of the present invention, the thermal conductor is composed of graphene and carbon nanotubes, and the surface is modified with dopamine.

[0013] In any embodiment of the present invention, the thermal conductor is composed of graphene and carbon nanotubes in a weight ratio of 1 to 2:1, and the surface is modified with dopamine.

[0014] In any embodiment of the present invention, the antioxidant consists of L60 and microcrystalline wax.

[0015] In any embodiment of the present invention, the antioxidant consists of L60 and microcrystalline wax in a weight ratio of 3 to 1:1, for example, the antioxidant consists of L60 and microcrystalline wax in a weight ratio of 3:1, 2:1, or 1:1.

[0016] In any embodiment of the present invention, the reinforcing agent is carbon black; and / or the vulcanizing agent is sulfur; and / or the accelerator is benzothiazole disulfide (DM); and / or the activator is composed of zinc oxide and stearic acid in a weight ratio of 1:0.5 to 1.5.

[0017] A second aspect of the present invention provides a rubber bushing made of the long-life vibration-damping rubber material.

[0018] A third aspect of the present invention provides a vehicle comprising the rubber bushing.

[0019] A fourth aspect of the present invention provides a method for preparing a rubber bushing, comprising the following steps:

[0020] Prepare rubber raw materials according to the above-mentioned long-life vibration-damping rubber material;

[0021] The above raw materials are made into rubber bushings.

[0022] The above rubber raw material is made into a rubber bushing comprising the following steps:

[0023] Adding graphene and carbon nanotubes into a dopamine alkaline solution, stirring and dispersing to obtain a suspension; vacuum freeze-drying the suspension to obtain a thermal conductor;

[0024] Put natural rubber and eucommia rubber into an internal mixer, add itaconate rubber after mixing evenly, and continue mixing; add heat conductive agent after mixing evenly, and then thinly pass through six times on an open mixer to obtain a masterbatch;

[0025] Adding an antioxidant, a vulcanizing agent, an accelerator and an active agent to the masterbatch at room temperature, mixing and discharging the materials after mixing evenly, to obtain a mixed rubber material;

[0026] The mixed rubber material is vulcanized on a flat vulcanizer at a vulcanization temperature of 140 to 150° C. and a vulcanization time of 30 to 60 minutes to obtain a rubber bushing.

[0027] Compared with the prior art, the present invention has at least the following beneficial effects:

[0028] Compared with existing rubber materials, the long-life vibration-damping rubber material provided by the present invention has higher tear strength, which can reach 45.3 kN / m; high thermal conductivity and improved anti-aging performance, thereby making the tensile fatigue life as high as 350,000 times. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] For simplicity, the present invention only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range. Similarly, any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0031] It should be noted that, in the description of the present invention, unless otherwise specified, "above" and "below" are inclusive numbers, and the meaning of "multiple" in "one or more" is two or more. Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.

[0032] In the description of the present invention, the description with reference to the terms "any embodiment / method", "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments / methods or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, without contradiction.

[0033] The above summary of the invention of the present invention is not intended to describe each disclosed embodiment or each implementation in the present invention. The following description more specifically illustrates exemplary embodiments. These embodiments can be used in various combinations. In each example, the enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0034] Long life vibration damping rubber material

[0035] As described in the background technology, natural rubber is easy to age and has a short material life; due to the lack of large steric hindrance groups in its own molecular chain, the damping and vibration reduction performance is poor, and the automobile chassis rubber bushing produced reduces the comfort and stability of the whole vehicle. Although eucommia rubber has the advantages of good dynamic fatigue performance and low heat generation, the prior art believes that when eucommia rubber and natural rubber are mixed, eucommia rubber exists in the natural rubber matrix in a sheet form, which will reduce the tear strength of the rubber material and lead to a decrease in fatigue performance.

[0036] The inventors have found that the blending effect of Eucommia rubber and natural rubber is related to the dispersion degree of Eucommia rubber in the natural rubber system. When the amount of Eucommia rubber is small, no continuous phase is formed in the system. It is mainly distributed in the natural rubber system in the form of nano-scale small crystal island phase structure, which can be used as an active filler of natural rubber, inhibiting the crack propagation rate to a certain extent. At this stage, the tear strength of natural rubber will not decrease significantly, and may even increase. When the amount of Eucommia rubber increases to a certain amount, the nano-scale crystals of Eucommia rubber gradually disappear due to shearing during mixing, forming a dual continuous phase, and the tear strength of rubber begins to decrease. This is the reason why Eucommia rubber exists in the natural rubber matrix in the form of sheets in the prior art.

[0037] The present invention controls the eucommia rubber to account for 10wt% to 25wt% of the total raw rubber. The eucommia rubber does not form a continuous phase in a flaky form in the rubber matrix, but is mainly distributed in the matrix in the form of a nano-scale small crystal island phase structure. It can be used as an active filler for itaconate rubber and natural rubber, and can inhibit the crack propagation rate to a certain extent. Therefore, compared with natural rubber, the tear strength of the rubber material of the present invention will not be significantly reduced, but will be increased.

[0038] Based on this, the present invention provides a long-life vibration-damping rubber material and its preparation method and application. Compared with natural rubber, the tensile fatigue life and damping performance of the rubber material are significantly improved, and the rubber bushing produced has excellent vibration reduction and fatigue durability. Compared with the modification idea of ​​blending natural rubber and synthetic rubber in the prior art, the present invention blends natural rubber with bio-based rubber, which is green and environmentally friendly.

[0039] The long-life vibration-damping rubber material provided by the present invention is prepared by mixing rubber raw materials, wherein the rubber raw materials include, by weight percentage:

[0040]

[0041] The raw rubber consists of natural rubber, itaconate rubber and eucommia rubber, wherein the eucommia rubber accounts for 10wt% to 25wt% of the total raw rubber, the itaconate rubber accounts for 30wt% to 70wt% of the total raw rubber, and the natural rubber accounts for 20wt% to 45wt% of the total raw rubber.

[0042] The raw rubber of the present invention is composed of natural rubber, itaconate rubber and eucommia rubber. At room temperature, the eucommia rubber exists in the form of nano crystals in the matrix, which can hinder the initiation and expansion of cracks; the eucommia rubber can hinder the diffusion of the medium and inhibit the aging of the rubber material; at the same time, the nano crystals formed by the eucommia rubber have a lower melting point than natural rubber, and can absorb a large amount of heat during the melting process, reducing the destructive effect of high temperature on the molecular structure of the rubber material. The ester group contained in the itaconate rubber can form a hydrogen bond network with various additives inside the rubber material, limit the movement of the molecular chain inside the rubber material, increase the internal friction of the rubber material, thereby increasing the damping factor of the rubber material and improving the vibration reduction performance of the rubber material.

[0043] The present invention controls the eucommia rubber in the raw rubber to account for 10wt% to 25wt% of the total raw rubber, which can prevent the eucommia rubber from forming a continuous phase in a sheet in the matrix, resulting in tearing along the surface of the sheet structure during the tearing process of the rubber material, thereby reducing the tear strength of the rubber. More importantly, the eucommia rubber accounts for 10wt% to 25wt% of the total raw rubber, and the nano-scale small crystals formed by the eucommia rubber can play the role of active filler, hinder the initiation and expansion of cracks, and thus improve the tear strength of the rubber material.

[0044] Furthermore, the rubber raw material contains 60 wt% to 62 wt% of raw rubber by weight. If the raw rubber content is controlled within the above range, the rubber material can be guaranteed to have sufficient tear strength and vibration reduction performance.

[0045] In some embodiments of the present invention, the thermal conductor is composed of graphene and carbon nanotubes, and the surface is modified with dopamine; preferably, the thermal conductor is composed of graphene and carbon nanotubes in a weight ratio of 1 to 2:1, and the surface is modified with dopamine. The present invention introduces a thermal conductor into the rubber material, and the unique network structure of the thermal conductor makes the rubber material have excellent mechanical properties and thermal conductivity. The high thermal conductivity can conduct the heat generated by the rubber material, slow down the aging of the rubber material, and thus extend the service life of the rubber material. The present invention performs dopamine modification on the surface of graphene and carbon nanotubes in advance, which can solve the problem that graphene and carbon nanotubes are difficult to disperse in the rubber matrix. The surface of dopamine contains functional groups such as hydroxyl, amino, and catechol groups, which have a strong modification effect. The increase in specific surface area and the rich active groups can make them evenly dispersed in the rubber matrix. The unique network structure makes the prepared rubber material have excellent mechanical properties and thermal conductivity. The thermal conductor of the present invention uses graphene and carbon nanotubes at the same time because: one-dimensional graphene and two-dimensional carbon nanotubes are modified by dopamine to form a three-dimensional hybrid stacking system, which has a synergistic enhancement effect on the rubber matrix, and the thermal conductivity and heat dissipation performance of the three-dimensional hybrid stacking system is improved.

[0046] In some embodiments of the present invention, the antioxidant is composed of L60 and microcrystalline wax. Preferably, the antioxidant is composed of L60 and microcrystalline wax in a weight ratio of 3 to 1:1. The present invention adopts a combination of chemical anti-aging and physical anti-aging to significantly improve the aging performance of rubber materials and effectively extend the service life of rubber materials. The main component of the chemical antioxidant L60 is derived from lignin. Its structure contains a large number of functional groups such as aromatic groups, methoxy groups, ether bonds, and phenolic hydroxyl groups. It can react with high molecular oligomers in raw rubber, bond the anti-aging groups to the oligomers, and exert a lasting protective effect. The migration rate of the physical antioxidant micro-60 crystalline wax in the rubber matrix is ​​relatively slow, forming a longer protective film and having a better protective effect.

[0047] The present invention does not limit the type of reinforcing agent. In some embodiments, the reinforcing agent can be selected from at least one of carbon black N110, N220, and N330.

[0048] The present invention does not limit the type of the vulcanizing agent. In some embodiments, the vulcanizing agent can be selected from precipitated sulfur with an average particle size of 1 to 5 microns.

[0049] The present invention does not limit the type of the accelerator. In some embodiments, the accelerator can be selected from at least one of benzothiazole disulfide, 2-thiolbenzothiazole, and 2-thiolbenzothiazole zinc salt.

[0050] The present invention does not limit the type of active agent. In some embodiments, the active agent can be selected from at least one of zinc oxide and stearic acid. Preferably, the active agent is composed of zinc oxide and stearic acid in a weight ratio of 1:0.5 to 1.5.

[0051] The long-life vibration-damping rubber material provided by the invention adopts eucommia rubber and itaconate rubber to replace natural rubber, thereby alleviating the problem of insufficient natural rubber resources.

[0052] Rubber bushing

[0053] Since the long-life vibration-damping rubber material has a long fatigue life and a high damping factor, it is particularly suitable for manufacturing rubber bushings, especially bushings for heavy truck chassis.

[0054] The present invention makes the long-life vibration-damping rubber material into a rubber bushing and conducts performance tests, and finds that the tensile fatigue life can reach 290,000 to 350,000 times, and the thermal conductivity is 0.39 to 0.42 W / m·K.

[0055] vehicle

[0056] Applying the above bushing to a vehicle can improve the safety of the vehicle, reduce the frequency of replacing the rubber bushing, and enhance the customer experience. For example, a vehicle includes a rubber bushing made of a long-life vibration-damping rubber material. The long-life vibration-damping rubber material can be used to prepare rubber bushings at any part of the vehicle, and is particularly suitable for thrust rod bushings or guide arm bushings that have high requirements for tensile strength and tear strength.

[0057] Preparation method of rubber bushing

[0058] The method for preparing a rubber bushing provided by the present invention comprises the following steps:

[0059] Prepare rubber raw materials according to the above-mentioned long-life vibration-damping rubber material;

[0060] The above raw materials are made into rubber bushings.

[0061] The above rubber raw material is made into a rubber bushing comprising the following steps:

[0062] Adding graphene and carbon nanotubes into a dopamine alkaline solution, stirring and dispersing to obtain a suspension; vacuum freeze-drying the suspension to obtain a thermal conductor;

[0063] Put natural rubber and eucommia rubber into an internal mixer, mix for 1 to 2 minutes, then add itaconate rubber, and continue mixing for 1 to 2 minutes; after mixing evenly, add a heat conductive agent, and then thinly pass six times on an open mixer to obtain a masterbatch;

[0064] Adding antioxidant, vulcanizing agent, accelerator and activator to the masterbatch at room temperature, mixing for 5 to 10 minutes and then discharging to obtain a mixed rubber material;

[0065] The mixed rubber material is vulcanized on a flat vulcanizer at a vulcanization temperature of 140 to 150° C. and a vulcanization time of 30 to 60 minutes to obtain a rubber bushing.

[0066] The method first modifies the surface of the thermal conductor with dopamine, and then adds it into raw rubber for mixing. This can solve the problem that graphene and carbon nanotubes are difficult to disperse in the rubber matrix, and the one-dimensional graphene and the two-dimensional carbon nanotubes can be modified with dopamine to prepare a three-dimensional hybrid stacking system of thermal conductors in advance, which can be added to the rubber matrix to synergistically strengthen the matrix. Finally, other additives are added, vulcanization is carried out, and finally a rubber bushing is obtained.

[0067] Example

[0068] The following are examples of the present invention. The examples described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the art or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained commercially. The carbon black used in the examples is N330.

[0069] Example 1

[0070] The rubber material provided in this embodiment is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 20 parts of natural rubber, 60 parts of itaconate rubber, 10 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 2 parts of graphene, 1 part of carbon nanotubes, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 1.5 parts of stearic acid.

[0071] This embodiment adopts the following preparation method to prepare rubber material:

[0072] The weighed graphene and carbon nanotubes were added to a 2 g / L dopamine alkaline solution, and the mixture was stirred and dispersed for 2 h to obtain a suspension; the suspension prepared above was placed in a vacuum freeze drying oven and dried for 12 h;

[0073] Put natural rubber and eucommia rubber into an internal mixer, mix for 2 minutes, then add itaconate rubber and continue mixing for 2 minutes;

[0074] After mixing evenly in an internal mixer, add dried graphene and carbon nanotubes to prepare a masterbatch, and place it at room temperature for 24 hours;

[0075] Add antioxidant, vulcanizing agent, accelerator and activator to the cooled masterbatch, mix for 10 minutes and then discharge;

[0076] The mixed rubber prepared on the internal mixer is thinly passed three times on an open mixer to form sheets;

[0077] The prepared mixed rubber material was vulcanized on a flat vulcanizer at a vulcanization temperature of 155° C. and a vulcanization time of 40 min to obtain a rubber material.

[0078] Take the corresponding standard samples of the rubber materials prepared above and test them:

[0079] Test the tensile properties of rubber materials according to GB / T528;

[0080] Test the tearing properties of rubber materials according to GB / T529;

[0081] Test the Shore A hardness of rubber materials according to GB / T531;

[0082] Test the compression permanent deformation of rubber materials according to GB / T7759;

[0083] The damping coefficient of the material was tested using a dynamic mechanical analyzer (benzothiazyl disulfide A).

[0084] The tensile fatigue life of rubber materials is tested according to GB / T1688.

[0085] The vulcanized rubber material was cut into small discs with a thickness of 2 mm and a diameter of 30 mm, and the thermal conductivity of the rubber material was measured using a DRL-Ⅲ thermal conductivity tester.

[0086] Example 2

[0087] The rubber material provided in this embodiment is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 40 parts of natural rubber, 30 parts of itaconate rubber, 20 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 2 parts of graphene, 1 part of carbon nanotubes, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 1.5 parts of stearic acid.

[0088] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0089] Example 3

[0090] The rubber material provided in this embodiment is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 30 parts of natural rubber, 50 parts of itaconate rubber, 15 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 2 parts of graphene, 1 part of carbon nanotubes, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 1.5 parts of stearic acid.

[0091] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0092] Example 4

[0093] The rubber material provided in this embodiment is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 20 parts of natural rubber, 60 parts of itaconate rubber, 20 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 3 parts of graphene, 2 parts of carbon nanotubes, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 1.5 parts of stearic acid.

[0094] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0095] Comparative Example 1

[0096] The vibration-damping rubber material provided in this comparative example is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 100 parts of natural rubber, 50 parts of carbon black, 4 parts of sulfur, 1 part of accelerator benzothiazole disulfide, 3 parts of zinc oxide, 1.5 parts of stearic acid, and 2 parts of antioxidant 4010NA.

[0097] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0098] Comparative Example 2

[0099] The vibration-damping rubber material provided in this comparative example is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 70 parts of natural rubber, 30 parts of butadiene rubber, 50 parts of carbon black, 4 parts of sulfur, 3 parts of zinc oxide, 1.5 parts of stearic acid, and 2 parts of antioxidant 4010NA.

[0100] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0101] Comparative Example 3

[0102] The difference between this comparative example and Example 1 is that less graphene and carbon nanotubes are added in this comparative example.

[0103] The vibration-damping rubber material provided in this comparative example is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 20 parts of natural rubber, 60 parts of itaconate rubber, 10 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 5 parts of stearic acid.

[0104] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0105] Comparative Example 4

[0106] The only difference between this comparative example and Example 1 is that in this comparative example, the carbon nanotubes are replaced by graphene of equal mass.

[0107] The vibration-damping rubber material provided in this comparative example is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 20 parts of natural rubber, 60 parts of itaconate rubber, 10 parts of eucommia rubber, 40 parts of carbon black, 3 parts of antioxidant L60, 1 part of microcrystalline wax, 3 parts of graphene, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 5 parts of stearic acid.

[0108] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0109] Comparative Example 5

[0110] The difference between this comparative example and Example 1 is that in this comparative example, the microcrystalline wax is replaced by an antioxidant L60 of equal mass.

[0111] The rubber material provided in this comparative example is mixed with rubber raw materials, and the rubber raw materials are composed of the following raw materials in weight fractions: 20 parts of natural rubber, 60 parts of itaconate rubber, 10 parts of eucommia rubber, 40 parts of carbon black, 4 parts of antioxidant L60, 2 parts of graphene, 1 part of carbon nanotubes, 3 parts of sulfur, 1 part of benzothiazole disulfide, 3 parts of zinc oxide, and 5 parts of stearic acid.

[0112] The preparation method and characterization test method of the rubber material are the same as those in Example 1.

[0113] Table 1 Performance test data of rubber materials prepared in Examples 1 to 4 and Comparative Examples 1 to 5

[0114]

[0115]

[0116] From Table 1, it can be seen that the mechanical properties of the rubber materials provided in Examples 1 to 4 of the present invention at room temperature do not show a significant decrease, but are improved compared with the ordinary natural rubber material in Comparative Example 1. In addition, the damping factor, tensile fatigue life, thermal conductivity and thermal aging properties of the rubber materials are significantly improved. The improvement of these material properties plays a vital role in long-life rubber bushings.

[0117] From the comparison between Comparative Examples 3 and 4 and Example 1, the tensile fatigue life of Comparative Example 3 without adding a thermal conductor is significantly reduced, and the tensile fatigue life of Comparative Example 4 with only adding graphene as a thermal conductor is also far inferior to that of Example 1 with adding both graphene and carbon nanotubes as thermal conductors. In addition, the thermal conductivity of Comparative Example 3 is also inferior to that of Comparative Example 4 and Example 1. It is speculated that this is because the high thermal conductivity of Comparative Example 4 and Example 1 can conduct the heat generated by the rubber material, slow down the aging of the rubber material, and thus extend the service life of the rubber material. The reason why the thermal conductivity and tensile fatigue life of Comparative Example 4 are inferior to those of Example 1 is speculated to be that the one-dimensional graphene and the two-dimensional carbon nanotubes in Example 1 form a three-dimensional hybrid stacking system through dopamine modification, and the interconnected graphene and carbon nanotubes improve the thermal conductivity and have a synergistic enhancement effect on the rubber matrix, thereby improving the tensile fatigue life of the rubber material.

[0118] From the comparison between Comparative Example 5 and Example 1, it can be seen that Comparative Example 5 only uses one antioxidant, antioxidant L60, and the tensile fatigue life is seriously reduced compared with Example 1. It is speculated that this is because the migration rate of the physical antioxidant microcrystalline wax used in Example 1 in the rubber matrix is ​​relatively slow, forming a longer protective film and having a better protective effect. The chemical antioxidant in Example 1 still has a good protective effect after failure.

[0119] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A long-life vibration-damping rubber material, characterized in that: The long-life vibration-damping rubber material is prepared by mixing rubber raw materials, and the rubber raw materials, measured by weight percentage, include: The raw rubber consists of natural rubber, itaconate rubber and eucommia rubber, wherein the eucommia rubber accounts for 10wt% to 25wt% of the total raw rubber, the itaconate rubber accounts for 30wt% to 70wt% of the total raw rubber, and the natural rubber accounts for 20wt% to 45wt% of the total raw rubber.

2. The long-life vibration-damping rubber material according to claim 1, characterized in that: The thermal conductor consists of graphene and carbon nanotubes, and is surface-modified with dopamine.

3. The long-life vibration-damping rubber material according to claim 2, characterized in that: The thermal conductor consists of graphene and carbon nanotubes in a weight ratio of 1 to 2:1, and is surface-modified with dopamine.

4. The long-life vibration-damping rubber material according to claim 1, characterized in that: The antioxidant consists of L60 and microcrystalline wax.

5. The long-life vibration-damping rubber material according to claim 4, characterized in that: The antioxidant consists of L60 and microcrystalline wax in a weight ratio of 3 to 1:

1.

6. The long-life vibration-damping rubber material according to claim 1, characterized in that: The reinforcing agent is carbon black; and / or, The vulcanizing agent is sulfur; and / or, The accelerator is benzothiazole disulfide; and / or, The active agent consists of zinc oxide and stearic acid in a weight ratio of 1:0.5-1.

5.

7. A rubber bushing, characterized in that: Made of the long-life vibration-damping rubber material according to any one of claims 1 to 6.

8. A vehicle, characterized in that: Comprising the rubber bushing as claimed in claim 7.

9. A method for preparing a rubber bushing, characterized in that: The following steps are involved: Prepare rubber raw materials according to the long-life vibration-damping rubber material of claims 1 to 6; The rubber raw material is made into a rubber bushing.

10. The method for preparing a rubber bushing according to claim 9, characterized in that: The above rubber raw material is made into a rubber bushing comprising the following steps: Adding graphene and carbon nanotubes into a dopamine alkaline solution, stirring and dispersing to obtain a suspension; vacuum freeze-drying the suspension to obtain a thermal conductor; Put natural rubber and eucommia rubber into an internal mixer, add itaconate rubber after mixing evenly, and continue mixing; add heat conductive agent after mixing evenly, and then thinly pass through six times on an open mixer to obtain a masterbatch; Adding an antioxidant, a vulcanizing agent, an accelerator and an activator to the masterbatch at room temperature, mixing and discharging the materials after mixing evenly, to obtain a mixed rubber material; The mixed rubber material is vulcanized on a flat vulcanizer at a vulcanization temperature of 140 to 150° C. and a vulcanization time of 30 to 60 minutes to obtain a rubber bushing.