Recycled plastic for storage battery bottom shell and preparation method thereof
By introducing modified elastomers and modified high barrier aids into recycled ABS plastics, the characteristics of hydroxyl groups and graphene oxide are used to solve the problem of reduced performance of recycled ABS plastics during thermal oxidation, and significantly improve their anti-oxidation and barrier performance.
Patent Information
- Application Number
- CN202411057986.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The oxidation reaction of recycled ABS plastic in existing battery shells accelerates when heated, resulting in a degradation of performance. How to improve the application performance of recycled plastics is a technical problem.
Using modified elastomers and modified high barrier additives, the oxidation resistance and barrier properties of recycled plastics are enhanced by introducing epoxy groups and graphene oxide. The hydroxyl groups in the modified elastomer form hydrogen bonds with the oxidation decomposition products. , the graphene oxide modified with high barrier additives enhances mechanical properties and film formation.
It improves the strength, toughness and oxidation resistance of recycled plastics, extends the transmission path of gas molecules, significantly reduces oxygen transmittance, enhances barrier properties, and extends the stability of the molecular chain.
Smart Images

Figure BDA0004976980590000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to recycled plastic for a battery bottom shell and a preparation method thereof. Background Art
[0002] Recycled plastic refers to plastic products discarded from daily life and production that are collected, sorted, cleaned, and crushed through physical or chemical methods, and then transformed into reusable plastics through processes such as melting and reshaping. With the continuous development of the battery manufacturing industry, various new energy batteries are widely used in electric vehicles, energy storage equipment, portable electronic devices and other fields, making the battery manufacturing industry have a huge demand for plastics. Therefore, waste plastics can be recycled and used in the production of battery shells. This not only saves resources, but also reduces environmental pollution caused by waste.
[0003] At present, the material of battery shell is usually ABS plastic. ABS plastic is a ternary copolymer formed by the copolymerization of three monomers: acrylonitrile, butadiene and styrene, and has good processing performance. However, in the molecular structure of ABS plastic, butadiene as the rubber phase contains unsaturated double bonds, which will accelerate the oxidation reaction with oxygen when heated, resulting in the breakage of the copolymer molecular chain and the generation of oxygen-containing groups such as carboxyl and aldehyde groups. In addition, repeated processing will further accelerate its oxidation reaction, resulting in the reduction of the performance of the recycled plastic of the battery bottom shell. Therefore, how to improve the application of recycled plastics in battery shells is a technical problem that needs to be solved at present. Summary of the invention
[0004] The object of the present invention is to provide a recycled plastic for a battery bottom shell and a preparation method thereof, so as to solve the problems in the background technology.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A recycled plastic for a battery bottom shell, comprising the following raw materials in parts by weight:
[0007] 100-110 parts of waste ABS plastic, 6-10 parts of modified elastomer, 0.5-1 parts of curing agent, 0.3-0.6 parts of defoaming agent, 8-12 parts of modified high barrier additive, 15-20 parts of high impact polystyrene;
[0008] The modified elastomer is prepared by the following steps:
[0009] A1. Add SIS copolymer to cyclohexane, stir and dissolve, then dropwise add meta-chloroperbenzoic acid solution at 60°C, heat to 70-75°C, reflux for 1.5-2h, cool, place in anhydrous methanol and let stand for sedimentation, then dissolve in tetrahydrofuran and let stand for precipitation, repeat sedimentation for several times, filter and dry to obtain epoxidation intermediate; use cyclohexane as solvent, adopt meta-chloroperbenzoic acid epoxidation method, combine the peroxy group in meta-chloroperbenzoic acid with the C=C double bond in SIS copolymer, and introduce epoxy group into the molecular chain of SIS copolymer;
[0010] A2. Add the epoxidation intermediate to tetrahydrofuran, stir and dissolve, then add deionized water and zirconium chloride in sequence, react at 20-25°C for 3-3.5h, then place in anhydrous ethanol for precipitation, and then filter, wash with anhydrous ethanol, and dry to obtain a modified elastomer; use zirconium chloride as a catalyst and deionized water as a nucleophilic reagent to attack the epoxy group of the epoxidation intermediate to obtain a hydroxylated modified elastomer.
[0011] Furthermore, the usage ratio of the cyclohexane, SIS copolymer and meta-chloroperbenzoic acid solution is 80 mL: 6-8 g: 10-15 mL; the meta-chloroperbenzoic acid solution is prepared by dissolving 4-6 g of meta-chloroperbenzoic acid in 20 mL of tetrahydrofuran.
[0012] Furthermore, the usage ratio of tetrahydrofuran, epoxidation intermediate, deionized water and zirconium chloride is 70mL:4-8g:1-3mL:2g.
[0013] Furthermore, the modified high barrier additive is prepared by the following steps:
[0014] B1. Add graphene oxide to anhydrous ethanol, stir and mix, and then ultrasonically disperse for 30 minutes, then add tannic acid aqueous solution, stir and react for 1-2 hours at room temperature, and then wash with deionized water and dry to obtain modified graphene oxide; the aromatic structure in tannic acid is adsorbed on the surface of graphene oxide through π-π conjugation to obtain modified graphene oxide with tannic acid loaded on the surface;
[0015] B2. Add polyvinyl alcohol to deionized water, stir and dissolve at 80-90°C, cool, dropwise add modified graphene oxide dispersion, stir and react for 2-3h, and let stand for 30min to obtain modified polyvinyl alcohol; various hydrogen bond combinations are formed between the oxygen-containing groups on the surface of the modified graphene oxide and the hydroxyl groups on the polyvinyl alcohol molecular chain to obtain modified polyvinyl alcohol grafted with graphene oxide.
[0016] Furthermore, the dosage ratio of the anhydrous ethanol, graphene oxide and tannic acid aqueous solution is 50mL:0.05-2g:10mL; the tannic acid aqueous solution is composed of tannic acid and deionized water in a volume ratio of 0.5-1:30.
[0017] Furthermore, the usage ratio of the deionized water, polyvinyl alcohol and modified graphene oxide dispersion is 70 mL: 6-7 g: 15-30 mL; the modified graphene oxide dispersion is prepared by dispersing 2-5 g of modified graphene oxide in 30 mL of deionized water.
[0018] A recycled plastic for a battery bottom shell is prepared by the following steps:
[0019] Waste ABS plastic, modified elastomer, curing agent, defoaming agent, modified high barrier additive and high impact polystyrene are added into a high-speed mixer for stirring and mixing, and then added into a screw extruder for extrusion. After cooling and pelletizing, recycled plastic for battery bottom shell is obtained.
[0020] Beneficial effects of the present invention:
[0021] The modified elastomer of the present invention contains abundant hydroxyl groups. When blended with waste ABS plastic, the hydroxyl groups can be combined with the waste ABS plastic through hydrogen bonds, so that the modified elastomer is evenly dispersed on the molecular chains of the waste ABS plastic, thereby improving the compatibility of the modified elastomer with the waste ABS plastic and enhancing the strength and toughness of the obtained recycled plastic. Meanwhile, when the recycled plastic is decomposed and broken by thermal oxidation, the excess hydroxyl groups in the modified elastomer can chemically react with the carboxyl groups and carbonyl groups generated during the oxidative decomposition, and the broken molecular chains are reconnected through complex molecular chain winding, thereby playing the role of a "bridge" connection of the modified elastomer in the molecular chain breakage zone, thereby improving the antioxidant performance of the recycled plastic.
[0022] The surface of the modified high barrier auxiliary agent of the present invention is grafted with graphene oxide, which improves the surface roughness of the modified high barrier auxiliary agent molecules, enhances the mechanical bite effect between the modified high barrier auxiliary agent and the waste ABS plastic matrix, and improves the dispersibility of the modified high barrier auxiliary agent in the waste ABS plastic matrix. At the same time, the polyvinyl alcohol introduced into the modified high barrier auxiliary agent has excellent film-forming properties and can form a covering layer on the surface of the recycled plastic, effectively improving the barrier performance of the recycled plastic. At the same time, the graphene oxide with increased interlayer spacing can extend the permeation path of gas molecules such as oxygen and water vapor, further improving the barrier performance of the recycled plastic.
[0023] The present invention uses waste ABS plastic as a matrix and high-impact polystyrene as a reinforcement. By introducing a modified elastomer and a modified high-barrier additive, on the one hand, the permeation path of gas molecules on the surface of the recycled plastic can be extended, the permeability of gas molecules can be reduced, and the barrier performance of the recycled plastic can be improved. On the other hand, when a small amount of gas molecules permeate and the molecular chain is oxidatively broken, the hydroxyl groups in the modified elastomer can reconnect the broken molecular chains through hydrogen bonding. Under the synergistic effect of the two, the antioxidant performance of the prepared recycled plastic is further improved. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] This embodiment provides a modified elastomer, which is prepared by the following steps:
[0027] A1. Add 6 g of SI S copolymer to 80 mL of cyclohexane, stir and dissolve, then dropwise add 10 mL of a solution prepared by dissolving 4 g of m-chloroperbenzoic acid in 20 mL of tetrahydrofuran at 60 ° C, then heat to 70 ° C, reflux for 1.5 h, cool, place in anhydrous methanol and let stand for sedimentation, then dissolve in tetrahydrofuran and let the precipitate stand, repeat the sedimentation several times, then filter and dry to obtain an epoxidation intermediate;
[0028] A2. Add 4 g of the epoxidation intermediate to 70 mL of tetrahydrofuran, stir to dissolve, then add 1 mL of deionized water and 2 g of zirconium chloride in sequence, react at 20°C for 3 h, then place in anhydrous ethanol for precipitation, and then filter, wash with anhydrous ethanol, and dry to obtain a modified elastomer.
[0029] Example 2
[0030] This embodiment provides a modified elastomer, which is prepared by the following steps:
[0031] A1. Add 7 g of SIS copolymer to 80 mL of cyclohexane, stir and dissolve, then dropwise add 12 mL of a solution prepared by dissolving 5 g of m-chloroperbenzoic acid in 20 mL of tetrahydrofuran at 60 ° C, then heat to 72 ° C, reflux for 1.5 h, cool, place in anhydrous methanol and let stand for sedimentation, then dissolve in tetrahydrofuran and let the precipitate stand for several times, repeat the sedimentation several times, and then filter and dry to obtain an epoxidation intermediate;
[0032] A2. Add 6 g of the epoxidation intermediate to 70 mL of tetrahydrofuran, stir to dissolve, then add 2 mL of deionized water and 2 g of zirconium chloride in sequence, react at 23 °C for 3 h, then place in anhydrous ethanol for precipitation, and then filter, wash with anhydrous ethanol, and dry to obtain a modified elastomer.
[0033] Example 3
[0034] This embodiment provides a modified elastomer, which is prepared by the following steps:
[0035] A1. Add 8 g of SIS copolymer to 80 mL of cyclohexane, stir and dissolve, then dropwise add 15 mL of a solution prepared by dissolving 6 g of m-chloroperbenzoic acid in 20 mL of tetrahydrofuran at 60 ° C, then heat to 75 ° C, reflux for 2 h, cool, place in anhydrous methanol and let stand for sedimentation, then dissolve in tetrahydrofuran and let the precipitate stand for several times, repeat the sedimentation several times, and then filter and dry to obtain an epoxidation intermediate;
[0036] A2. Add 8 g of the epoxidation intermediate to 70 mL of tetrahydrofuran, stir to dissolve, then add 3 mL of deionized water and 2 g of zirconium chloride in sequence, react at 25 °C for 3.5 h, then place in anhydrous ethanol for precipitation, and then filter, wash with anhydrous ethanol, and dry to obtain a modified elastomer.
[0037] Example 4
[0038] This embodiment provides a modified high barrier additive, which is prepared by the following steps:
[0039] B1. Add 2 g of graphene oxide to 50 mL of anhydrous ethanol, stir and mix, and then ultrasonically disperse for 30 min. Then add 10 mL of an aqueous solution composed of tannic acid and deionized water in a volume ratio of 1:30, stir and react at room temperature for 2 h, and then wash with deionized water and dry to obtain modified graphene oxide;
[0040] B2. Add 7 g of polyvinyl alcohol to 70 mL of deionized water, stir and dissolve at 90°C, cool, and dropwise add 30 mL of a dispersion prepared by dispersing 5 g of modified graphene oxide in 30 mL of deionized water. Stir and react for 3 h, and then let stand for 30 min to obtain modified polyvinyl alcohol.
[0041] Example 5
[0042] This embodiment provides a modified high barrier additive, which is prepared by the following steps:
[0043] B1. Add 1 g of graphene oxide to 50 mL of anhydrous ethanol, stir and mix, and then ultrasonically disperse for 30 min. Then add 10 mL of an aqueous solution composed of tannic acid and deionized water in a volume ratio of 0.8:30, stir and react at room temperature for 1.5 h, and then wash with deionized water and dry to obtain modified graphene oxide;
[0044] B2. Add 6.5 g of polyvinyl alcohol to 70 mL of deionized water, stir and dissolve at 85°C, cool, and dropwise add 20 mL of a dispersion prepared by dispersing 3 g of modified graphene oxide in 30 mL of deionized water. Stir and react for 2.5 h, and let stand for 30 min to obtain modified polyvinyl alcohol.
[0045] Example 6
[0046] This embodiment provides a modified high barrier additive, which is prepared by the following steps:
[0047] B1. Add 2 g of graphene oxide to 50 mL of anhydrous ethanol, stir and mix, and then ultrasonically disperse for 30 min. Then add 10 mL of an aqueous solution composed of tannic acid and deionized water in a volume ratio of 1:30, stir and react at room temperature for 2 h, and then wash with deionized water and dry to obtain modified graphene oxide;
[0048] B2. Add 7 g of polyvinyl alcohol to 70 mL of deionized water, stir and dissolve at 90°C, cool, and dropwise add 30 mL of a dispersion prepared by dispersing 5 g of modified graphene oxide in 30 mL of deionized water. Stir and react for 3 h, and then let stand for 30 min to obtain modified polyvinyl alcohol.
[0049] Example 7
[0050] This embodiment provides a recycled plastic for a battery bottom shell, comprising the following steps:
[0051] 100 parts by weight of waste ABS plastic, 6 parts by weight of modified elastomer, 0.5 parts by weight of curing agent, 0.3 parts by weight of defoaming agent, 8 parts by weight of modified high barrier additive and 15 parts by weight of high impact polystyrene are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and after cooling and pelletizing, recycled plastic for battery bottom shell is obtained.
[0052] Example 8
[0053] This embodiment provides a recycled plastic for a battery bottom shell, comprising the following steps:
[0054] 105 parts by weight of waste ABS plastic, 8 parts by weight of modified elastomer, 0.8 parts by weight of curing agent, 0.5 parts by weight of defoaming agent, 10 parts by weight of modified high barrier additive and 18 parts by weight of high impact polystyrene are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and after cooling and pelletizing, recycled plastic for battery bottom shell is obtained.
[0055] Example 9
[0056] This embodiment provides a recycled plastic for a battery bottom shell, comprising the following steps:
[0057] 110 parts by weight of waste ABS plastic, 10 parts by weight of modified elastomer, 1 part by weight of curing agent, 0.6 parts by weight of defoaming agent, 12 parts by weight of modified high barrier additive and 20 parts by weight of high impact polystyrene are added into a high-speed mixer and stirred and mixed, then added into a screw extruder for extrusion, and after cooling and pelletizing, recycled plastic for battery bottom shell is obtained.
[0058] Comparative Example 1: The modified elastomer was replaced by an equal amount of SIS copolymer, and the rest were the same.
[0059] Comparative Example 2: No modified elastomer was added, and the rest was the same.
[0060] Comparative Example 3: An equal amount of the modified high barrier additive was replaced by polyvinyl alcohol, and the rest was the same.
[0061] Performance tests were performed on Examples 7 to 9 and Comparative Examples 1 to 3. Oxygen permeability test: at a temperature of 23° C. and a relative humidity of 50%, refer to GB / T 31354-2014; thermal oxygen aging test method: the sample was placed in a thermal oxygen aging tester for thermal oxygen aging, the thermal oxygen aging temperature was set to 100° C., the time was 28 days, and the impact strength and flexural strength before and after aging were recorded. The impact strength was referred to GB / T1043-2008, and the flexural strength was referred to GB / T9341-2008. The results are shown in Table 1:
[0062] Table 1
[0063]
[0064]
[0065] It can be seen from Table 1 that the recycled plastics for battery bottom shells prepared from modified elastomers and modified high barrier additives in Examples 7-9 have significantly lower oxygen permeability coefficients than the recycled plastics prepared from Comparative Examples 1-3, and have good barrier properties; at the same time, the impact strength and flexural strength before and after oxidation are higher than those of Comparative Examples 1-3, and have good oxidation resistance; in addition, compared with Comparative Examples 2 and 3, Example 7 has higher impact strength and flexural strength, indicating that under the synergistic effect of the modified elastomer and the modified high barrier additive, the recycled plastic prepared has better oxidation resistance.
[0066] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A recycled plastic for a battery bottom shell, It is characterized in that It includes the following raw materials in parts by weight: 100-110 parts of waste ABS plastic, 6-10 parts of modified elastomer, 0.5-1 parts of curing agent, 0.3-0.6 parts of defoaming agent, 8-12 parts of modified high barrier additive, 15-20 parts of high impact polystyrene; The modified elastomer is prepared by the following steps: A1. Add SIS copolymer to cyclohexane, stir and dissolve, then dropwise add meta-chloroperbenzoic acid solution at 60°C, then heat to 70-75°C, reflux for 1.5-2h, cool, place in anhydrous methanol and let stand for sedimentation, then dissolve in tetrahydrofuran and let the precipitate stand, repeat sedimentation several times, then filter and dry to obtain an epoxidation intermediate; A2. Add the epoxidation intermediate to tetrahydrofuran, stir to dissolve, then add deionized water and zirconium chloride in sequence, react at 20-25°C for 3-3.5h, then place in anhydrous ethanol for precipitation, filter, wash with anhydrous ethanol, and dry to obtain a modified elastomer.
2. The recycled plastic for battery bottom shell according to claim 1, It is characterized in that The dosage ratio of the cyclohexane, SIS copolymer and meta-chloroperbenzoic acid solution is 80 mL: 6-8 g: 10-15 mL; the meta-chloroperbenzoic acid solution is prepared by dissolving 4-6 g of meta-chloroperbenzoic acid in 20 mL of tetrahydrofuran.
3. The recycled plastic for battery bottom shell according to claim 1, It is characterized in that The usage ratio of tetrahydrofuran, epoxidation intermediate, deionized water and zirconium chloride is 70 mL: 4-8 g: 1-3 mL: 2 g.
4. The recycled plastic for battery bottom shell according to claim 1, It is characterized in that The modified high barrier additive is prepared by the following steps: B1. Add graphene oxide to anhydrous ethanol, stir and mix, and then disperse by ultrasonic for 30 minutes, then add tannic acid aqueous solution, stir and react at room temperature for 1-2 hours, and then wash with deionized water and dry to obtain modified graphene oxide; B2. Add polyvinyl alcohol to deionized water, stir and dissolve at 80-90° C., cool, dropwise add modified graphene oxide dispersion, stir and react for 2-3 hours, and then stand for 30 minutes to obtain modified polyvinyl alcohol.
5. The recycled plastic for battery bottom shell according to claim 4, It is characterized in that The dosage ratio of the anhydrous ethanol, graphene oxide and tannic acid aqueous solution is 50mL:0.05-2g:10mL; the tannic acid aqueous solution is composed of tannic acid and deionized water in a volume ratio of 0.5-1:
30.
6. The recycled plastic for battery bottom shell according to claim 4, It is characterized in that The usage ratio of the deionized water, polyvinyl alcohol and modified graphene oxide dispersion is 70 mL: 6-7 g: 15-30 mL; the modified graphene oxide dispersion is prepared by dispersing 2-5 g of modified graphene oxide in 30 mL of deionized water.
7. The method for preparing recycled plastic for battery bottom shell according to claim 1, It is characterized in that The following steps are involved: Waste ABS plastic, modified elastomer, curing agent, defoaming agent, modified high barrier additive and high impact polystyrene are added into a high-speed mixer for stirring and mixing, and then added into a screw extruder for extrusion. After cooling and pelletizing, recycled plastic for battery bottom shell is obtained.