Environment-friendly efficient lubricant for polyvinyl chloride and preparation method thereof
By combining epoxidized amide and silica oil, the problem of unstable compatibility and performance of lubricants for processing of polyvinyl chloride at high temperatures is solved, and efficient lubrication and enhancement of the mechanical properties and resistance of polyvinyl chloride is achieved. High temperature performance.
Patent Information
- Application Number
- CN202411245424.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lubricants for polyvinyl chloride processing have low compatibility and unstable performance at high temperatures, making it difficult to meet the processing needs in high temperature environments.
Using a combination of epoxidized amide and silicon amide oil, epoxy groups and imide groups are introduced during the preparation of epoxidized amide, and the polarity of polyvinyl chloride is reduced through silicon nitride oil to enhance its epoxy The compatibility of the amides forms an efficient lubricating layer, improving the mechanical properties and high temperature resistance of polyvinyl chloride.
The lubricating performance, wear resistance and high temperature resistance of polyvinyl chloride are significantly improved at high temperatures, the compatibility with processing equipment is enhanced, adhesion and wear are reduced, and the overall stability and flatness of the material are improved.
Smart Images

Figure BDA0005030541950000021 
Figure BDA0005030541950000031 
Figure BDA0005030541950000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricant processing for plastics, and in particular to an environmentally friendly and efficient lubricant for polyvinyl chloride and a preparation method thereof. Background Art
[0002] Polyvinyl chloride is the world's second largest general-purpose resin and the most widely used thermoplastic resin. Since the friction between polyvinyl chloride and between polyvinyl chloride melt and the metal surface of the processing machinery will reduce the viscous flow resistance of the melt, it is essential to add lubricants during the processing of polyvinyl chloride.
[0003] In recent years, research is moving towards more environmentally friendly and high-performance lubricants, with the focus shifting to lubricants with higher thermal and chemical stability, such as silicone compounds and fluorinated lubricants, which provide better performance under a wider range of operating conditions, especially at high temperatures and in harsh environments.
[0004] Prior art CN1522841A discloses a method for preparing a lubricant for polyvinyl chloride processing, which relates to a thermoplastic resin processing aid, in particular to a method for preparing a lubricant for polyvinyl chloride product molding processing. The lubricant is made of natural fats and oils as raw materials, which are hydrogenated at a hydrogen pressure of 5-6 MPa and a reaction temperature of 100-200°C after epoxidation to form triglycerides containing hydroxy fatty acids. Assuming that the weight of the PVC product is 100 parts, the lubricant is added to the PVC product at a ratio of 0.3-3.0 parts, and the use effect after molding is similar to that of adding hard castor oil.
[0005] Lubricating oil for polyvinyl chloride processing is obtained by epoxidation and hydrogenation treatment of natural fats and oils as raw materials. Although this lubricant containing triglycerides of hydroxy fatty acids has a certain lubricating effect, it is only processed with natural fats and oils as base materials. The compatibility of the obtained lubricating oil with polyvinyl chloride is low, and the fatty acid chain will decompose during high-temperature processing, causing the chemical structure of the oil to be destroyed and producing unstable by-products. The performance of the lubricant at high temperatures needs to be further improved. Summary of the invention
[0006] The object of the present invention is to provide an environmentally friendly and efficient lubricant for polyvinyl chloride and a preparation method thereof, so as to solve the technical problem in the prior art that the compatibility of lubricants with polyvinyl chloride materials and the high temperature resistance need to be further improved.
[0007] The object of the present invention can be achieved by the following technical scheme: an environmentally friendly and efficient lubricant for polyvinyl chloride, comprising the following raw material components in parts by weight: 10-20 parts of epoxidized amide and 15-40 parts of ammoniated silicone oil;
[0008] The preparation method of epoxidized amide is as follows: 20-25 parts of imidized polyamide, 3-5 parts of glacial acetic acid, 2-4 parts of hydrogen peroxide and 60-80 parts of N,N-dimethylformamide are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the epoxidized amide is obtained by post-treatment.
[0009] The reaction equation for synthesizing epoxidized amide is:
[0010]
[0011] In the formula,
[0012] The reaction principle for synthesizing epoxidized amide is as follows: under heating conditions, hydrogen peroxide and glacial acetic acid react to generate peroxy acid groups, which then undergo epoxidation reaction with unsaturated double bonds to prepare epoxidized amide.
[0013] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain epoxidized amide.
[0014] Furthermore, the preparation method of the imidized polyamide is as follows: 3-5 parts of N-hydroxysuccinimide, 1-2 parts of N,N-dicyclohexylcarbodiimide, 0.3-0.5 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reactor, reacted at room temperature for 0.5-1h, 20-30 parts of acidified polyamide are added into the reactor, the temperature of the reactor is increased to 40-50°C, the reaction is kept warm for 2-4h, and post-processed to obtain the imidized polyamide.
[0015] The reaction equation for synthesizing imidized polyamide is:
[0016]
[0017] In the formula,
[0018] The reaction principle of synthesizing imidized polyamide is as follows: NHS esterification occurs in the reaction, and the reaction uses the active intermediate NHS ester to convert carboxylic acid into its corresponding ester. In the reaction, N-hydroxysuccinimide and N,N-dicyclohexylcarboximide are first mixed to form an imide salt at room temperature, and then an acidified polyamide with a carboxyl group is added. At this time, the imide salt will be attacked by hydroxide ions and lose N,N-dicyclohexylcarboximide ions to form an imidized polyamide.
[0019] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain imidized polyamide.
[0020] Furthermore, the preparation method of the acidified polyamide is as follows: 20-30 parts of chain-extended fatty acid amide, 5-10 parts of 2,3-biphenyl maleic anhydride, 75-100 parts of dimethyl sulfoxide and 1-3 parts of aluminum chloride are weighed and added into a reactor, the temperature of the reactor is raised to 150-170° C., and the acidified polyamide is obtained by post-treatment.
[0021] The reaction equation for synthesizing acidified polyamide is:
[0022]
[0023] In the formula,
[0024] The reaction principle of synthesizing acidified polyamide is as follows: Lewis acid aluminum chloride catalyst protonates the anhydride to generate hydrogen oxide ions and anhydride intermediates, and the epoxy group attacks the carbonyl carbon of the anhydride intermediate through a nucleophilic addition reaction to form a ring-opening product to obtain the acidified polyamide.
[0025] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain acidified polyamide.
[0026] Furthermore, the preparation method of the chain-extended fatty acid amide is as follows: 10-15 parts of epoxidized amide, 5-8 parts of 2,6,10-trimethyl-2,6,10-pentadecatriene-14-one, 5-8 parts of (2E,4E)-5-(4-methoxy-2,3,6-trimethylphenyl)-3-methyl-2,4-pentadienal, 2-3 parts of γ-alumina and 30-40 parts of dimethyl sulfoxide are weighed by weight and added into a reactor, the temperature of the reactor is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the chain-extended fatty acid amide is obtained by post-treatment.
[0027] The reaction equation for synthesizing chain-extended fatty acid amide is:
[0028]
[0029] In the formula,
[0030] The reaction principle for synthesizing chain-extended fatty acid amide is as follows: secondary amine, aldehyde and ketone with aH react under acidic conditions, firstly generating an imine ion in the reaction, and then reacting with the enol form of the ketone to form a CC bond, thereby preparing the chain-extended fatty acid amide.
[0031] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain the chain-extended fatty acid amide.
[0032] Furthermore, the preparation method of epoxidized amide is as follows: 10-15 parts of modified fatty acid amide, 3-5 parts of glacial acetic acid, 2-4 parts of hydrogen peroxide and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reactor, the temperature of the reactor is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the epoxidized amide is obtained by post-treatment.
[0033] The reaction equation for synthesizing epoxidized amide is:
[0034]
[0035] The reaction principle for synthesizing epoxidized amide is as follows: under heating conditions, hydrogen peroxide and glacial acetic acid react to generate peroxy acid groups, which then undergo epoxidation reaction with unsaturated double bonds to prepare epoxidized amide.
[0036] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain epoxidized amide.
[0037] Furthermore, the preparation method of the modified fatty acid amide is as follows: 20-30 parts of 8,13-dimethyl-8,12-eicosenedioic acid, 5-10 parts of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, and 75-100 parts of dimethyl sulfoxide are weighed by weight and added into a reactor, stirred at room temperature for 5-10 minutes, the temperature of the reactor is lowered to 0-5°C, 1-2 parts of 1-hydroxybenzotriazole and 1-2 parts of dicyclohexylcarbodiimide are added thereto, the reaction is kept warm for 1-2 hours, and the modified fatty acid amide is obtained by post-treatment.
[0038] The reaction equation for synthesizing modified fatty acid amide is:
[0039]
[0040] The reaction principle of synthesizing modified fatty acid amide is as follows: 8,13-dimethyl-8,12-eicosenedioic acid reacts with carbodiimide to generate an active intermediate, and the amino group undergoes nucleophilic attack to generate a condensation product. Since the addition intermediate of the acid to carbodiimide in the first stage of the reaction is not stable, the addition of acylation catalyst 1-hydroxybenzotriazole makes the reaction stable and thorough, and finally an amidated polyurethane is obtained.
[0041] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain modified fatty acid amide.
[0042] Furthermore, the preparation method of ammoniated silicone oil is as follows: 20-30 parts of telomerized silicone oil, 6-8 parts of triaminosilane, 0.5-1.5 parts of chloroplatinic acid and 40-50 parts of xylene are weighed by weight and added into a reactor, the temperature of the reactor is increased to 50-60° C., and the ammoniated silicone oil is obtained by post-treatment.
[0043] The reaction equation for synthesizing aminated silicone oil is:
[0044]
[0045] The reaction principle of synthesizing aminated silicone oil is as follows: under the catalytic action of chloroplatinic acid, the unsaturated double bonds in the telomerized silicone oil and the silicon-hydrogen bonds in triaminosilane undergo a silylation addition reaction to prepare aminated silicone oil.
[0046] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is produced to obtain ammoniated silicone oil.
[0047] Further, the preparation method of telomerized silicone oil comprises the following steps:
[0048] A1, weigh 20-30 parts of methyl high hydrogen silicone oil, 3-5 parts of ammonium fluoride, 0.5-1.5 parts of silver fluoride and 40-50 parts of benzene by weight, add them into a reaction kettle, react at room temperature for 4-6 hours, and post-treat to obtain fluorinated silicone oil;
[0049] The reaction equation for synthesizing fluorinated silicone oil is:
[0050]
[0051] The reaction principle of synthesizing fluorinated silicone oil is as follows: the role of silver salt is to promote the activation of silicon-hydrogen bonds by providing fluoride ions to form active intermediates, and promote the reaction between silicon-hydrogen bonds and the fluorination reagent ammonium fluoride to obtain fluorinated silicone oil.
[0052] A2, weigh 8-10 parts of fluorinated silicone oil, 3-5 parts of tetramethyldivinyldisiloxane, 20-25 parts of 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane and 40-50 parts of ether by weight, add them into a reaction kettle, and stir at room temperature for 15-20 minutes to obtain a reaction precursor solution;
[0053] A3, weighing 20-30 parts of reaction precursor solution and 2-3 parts of 98wt% sulfuric acid solution by weight, adding them into the reaction kettle, keeping the temperature at room temperature for 8-10 hours to obtain a reaction solution;
[0054] A4. Add solid sodium bicarbonate to the reaction kettle containing the reaction solution until the pH of the reaction solution is 7-8, and then perform post-treatment to obtain telomerized silicone oil.
[0055] The reaction equation for synthesizing telomerized silicone oil is:
[0056]
[0057] The reaction principle of synthesizing telomerized silicone oil is as follows: under the action of concentrated sulfuric acid as an initiator, fluorinated silicone oil, tetramethyldivinyldisiloxane and tetramethyltetravinylcyclotetrasiloxane undergo telomerization reaction, with tetramethyldivinyldisiloxane serving as a telomerization agent, fluorinated silicone oil and tetramethyltetravinylcyclotetrasiloxane serving as main chain monomer substances, and finally telomerized silicone oil is prepared.
[0058] Furthermore, in step A1, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 80-100°C, and the reduced pressure distillation is performed until no liquid is produced to obtain fluorinated silicone oil; in step A4, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 80-100°C, and the reduced pressure distillation is performed until no liquid is produced to obtain polyurethane silicone oil.
[0059] The present invention also provides a method for preparing an environmentally friendly and efficient lubricant for polyvinyl chloride, which comprises adding epoxidized amide and ammoniated silicone oil into a reaction kettle and stirring them evenly to obtain the environmentally friendly and efficient lubricant for polyvinyl chloride.
[0060] The present invention has the following beneficial effects:
[0061] 1. In the process of preparing an environmentally friendly and efficient lubricant for polyvinyl chloride, the present invention first prepares a modified fatty acid, introduces an epoxy group through epoxidation and then performs chain extension, uses amide acidification and further esterification to obtain an imidized polyurethane, and further epoxidizes to obtain an epoxidized amide, which is more efficient while ensuring the lubrication effect and has certain environmental protection performance. The spatial structure of the polyvinyl chloride resin can be optimized at high temperature to achieve a certain plasticizing effect. At the same time, considering that the polarity of polyvinyl chloride is too strong, resulting in low compatibility with auxiliary materials such as lubricants, in order to reduce the polarity of polyvinyl chloride; the present invention It is clear that a nitrided silicone oil is obtained by fluorinating methyl high-hydrogen silicone oil, then polymerizing it with siloxane substances and then nitriding it. The nitrided silicone oil reduces the polarity of polyvinyl chloride at high temperature, enhances its compatibility with epoxidized amide, and cooperates with epoxidized urethane to enhance the mechanical properties of polyvinyl chloride materials. The lubricating layer formed by the nitrided silicone oil at high temperature reduces the adhesion of polyvinyl chloride materials and processing equipment, and improves the surface smoothness of polyvinyl chloride materials. By mixing epoxidized amide and nitrided silicone oil, an environmentally friendly and efficient lubricant is obtained, which improves the mechanical properties, wear resistance and high temperature resistance of polyvinyl chloride.
[0062] 2. In the process of preparing epoxidized amide, a long-chain fatty acid amide structure with carbon-carbon double bonds is obtained by polymerization. The fatty acid amide with the long-chain structure provides a basis for the lubricity and high temperature resistance of the material, and the staggered carbon-carbon double bonds in its structure also provide a basis for further modification of the fatty acid amide. The benzene ring on the chain structure further improves the mechanical properties of the long-chain fatty acid amide, and a large number of fluorine groups on it reduce the friction coefficient of the long-chain structure, thereby reducing wear and improving the lubrication effect while improving the thermal stability of the lubricant, so that it maintains its performance under high temperature environment; further, the carbon-carbon double bonds are converted into epoxy groups through epoxidation reaction to enhance the reactivity of the long-chain structure, and the chain extension reaction is carried out through secondary amino groups and aldehydes and ketones, which greatly improves the complexity of the side chains of the long-chain structure, and the large number of double bonds introduced provide a functional group basis for subsequent modification; the long-chain structure is further improved after further reaction with anhydride to undergo ring-opening acidification. The high complexity of the long-chain structure's branches, the introduced hydroxyl groups and double bonds enhance the reactivity of the long-chain structure, and provide a basis for further modification; further, the imide groups are introduced into the branches through esterification to further enhance the thermal stability of the long-chain structure, prevent it from degrading or failing at high temperatures, and at the same time enhance the lubrication effect of the long-chain structure, reduce friction and wear, improve lubrication efficiency, and enhance the overall stability of the long chain, making it more reliable under various conditions of use; finally, part of the double bonds in the long-chain structure are converted into epoxy groups through peracid catalysis, and the epoxy groups open the ring by reacting with the hydrogen chloride produced by the high-temperature cracking of polyvinyl chloride, and react with the active sites on the cracked polyvinyl chloride to cross-link, thereby achieving the effect of a hybrid polyvinyl chloride structure, and the carbon-carbon double bonds thereon undergo a Diels-Alder reaction with the multiple active sites produced by the cracking of polyvinyl chloride to form a ring structure, further improving the mechanical properties of polyvinyl chloride.
[0063] 3. In the process of preparing silicone nitride oil of the present invention, the activity of methyl high hydrogen silicone oil is reduced by fluorination, thereby reducing side reactions. At the same time, the low surface energy of the fluorine group further improves the lubrication performance and high temperature stability of the silicone oil; further, a polysilicone oil with a large number of carbon-carbon double bonds is generated through a polycondensation reaction, and its internal and end-capped carbon-carbon double bonds provide a basis for further modification and introduction of a large number of amino groups; further, a silicon group is further introduced while introducing amino groups through a hydrosilylation reaction, thereby increasing the silicon content in the silicone nitride oil and enhancing the lubrication performance of the silicone oil. The silicone nitride oil with an increased silicon content while reducing friction and wear has better thermal stability, can maintain its chemical properties and lubrication performance under high temperature conditions, is not easy to volatilize or degrade, and the silicone nitride oil reduces the adhesion of polyvinyl chloride to processing equipment at high temperatures, improves the flatness of the polyvinyl chloride surface, and reduces the polarity of polyvinyl chloride, thereby increasing the compatibility of polyvinyl chloride and auxiliary materials, further improving the performance of the polyvinyl chloride material. DETAILED DESCRIPTION
[0064] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] The methyl high hydrogen silicone oil used in the present invention is purchased from Anhui Mingyi Silicon Industry Co., Ltd., and the product is MY202 high hydrogen silicone oil.
[0066] Example 1
[0067] This embodiment provides a method for preparing an environmentally friendly and efficient lubricant for polyvinyl chloride, comprising the following steps:
[0068] S1. Preparation of chain-extended fatty acid amide
[0069] Weigh 14.0 g of 8,13-dimethyl-8,12-eicosenedioic acid, 4.0 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, and 40.0 g of dimethyl sulfoxide into a reactor, stir at room temperature for 5 min, lower the temperature of the reactor to 0° C., add 0.8 g of 1-hydroxybenzotriazole and 0.8 g of dicyclohexylcarbodiimide, and keep the reaction for 1 h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 80° C., and distill under reduced pressure until no liquid is produced to obtain 16.2 g of modified fatty acid amide;
[0070] 15.0 g of modified fatty acid amide, 3.6 g of glacial acetic acid, 2.4 g of hydrogen peroxide and 40.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 60° C. and the reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced to obtain 15.5 g of epoxidized amide;
[0071] 14.0 g of epoxidized amide, 5.0 g of 2,6,10-trimethyl-2,6,10-pentadecatriene-14-one, 5.0 g of (2E, 4E)-5-(4-methoxy-2,3,6-trimethylphenyl)-3-methyl-2,4-pentadienal, 2.4 g of γ-alumina and 40.0 g of dimethyl sulfoxide were weighed and added into a reactor. The temperature of the reactor was raised to 60°C and the reaction was kept warm for 2 hours. After the reactor was cooled to room temperature, the reaction solution was added into a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced to obtain 23.5 g of extended chain fatty acid amide.
[0072] S2. Preparation of epoxidized amide
[0073] 21.0 g of chain-extended fatty acid amide, 8.0 g of 2,3-biphenyl maleic anhydride, 80.0 g of dimethyl sulfoxide and 2.0 g of aluminum chloride were weighed and added to a reactor. The temperature of the reactor was raised to 150° C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80° C., and distilled under reduced pressure until no liquid was produced, to obtain 27.3 g of acidified polyamide;
[0074] 3.5 g of N-hydroxysuccinimide, 1.5 g of N,N-dicyclohexylcarbodiimide, 0.5 g of triethylamine and 32.0 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 0.5 h, 20.0 g of acidified polyamide was added to the reactor. The temperature of the reactor was raised to 40° C. and the reaction was kept warm for 24 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced to obtain 23.2 g of imidized polyamide;
[0075] 20.0 g of imidized polyamide, 4.0 g of glacial acetic acid, 2.5 g of hydrogen peroxide and 75.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 60°C and kept warm for 2 hours. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced to obtain 21.2 g of epoxidized amide.
[0076] S3. Preparation of silicon nitride oil
[0077] 9.0 g of methyl high hydrogen silicone oil, 2.3 g of ammonium fluoride, 0.5 g of silver fluoride and 20.0 g of benzene were weighed and added to a reactor, and reacted at room temperature for 4 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced, to obtain 9.6 g of fluorinated silicone oil;
[0078] 8.0 g of fluorinated silicone oil, 5.0 g of tetramethyldivinyldisiloxane, 23.0 g of 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane and 50.0 g of ether were weighed and added into a reaction kettle, and stirred at room temperature for 15 min to obtain 86.0 g of reaction precursor solution;
[0079] Weigh 85.0g of the reaction precursor solution and 8.5g of 98wt% sulfuric acid solution into a reactor, and keep the reaction at room temperature for 8h to obtain a reaction solution. Add solid sodium bicarbonate to the reaction solution until the pH of the reaction solution is 7. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 80°C, and distill under reduced pressure until no liquid is produced to obtain 32.3g of telomerized silicone oil;
[0080] 30.0 g of polysilicone oil, 12.0 g of triaminosilane, 1.5 g of chloroplatinic acid and 75.0 g of xylene were weighed and added to a reactor. The temperature of the reactor was raised to 50°C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced to obtain 41.2 g of ammoniated silicone oil.
[0081] S4. Preparation of lubricant
[0082] 18.0 g of epoxidized amide and 36.0 g of aminated silicone oil were added into a reaction kettle and stirred evenly to obtain a lubricant for polyvinyl chloride.
[0083] Example 2
[0084] This embodiment provides a method for preparing an environmentally friendly and efficient lubricant for polyvinyl chloride, comprising the following steps:
[0085] S1. Preparation of chain-extended fatty acid amide
[0086] Weigh 25.0 g of 8,13-dimethyl-8,12-eicosenedioic acid, 9.0 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, and 80.0 g of dimethyl sulfoxide into a reactor, stir at room temperature for 10 min, lower the temperature of the reactor to 5° C., add 1.0 g of 1-hydroxybenzotriazole and 1.0 g of dicyclohexylcarbodiimide, and keep the reaction for 2 h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 100° C., and distill under reduced pressure until no liquid is produced to obtain 16.4 g of modified fatty acid amide;
[0087] 15.0 g of modified fatty acid amide, 4.2 g of glacial acetic acid, 2.1 g of hydrogen peroxide and 36.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and the reaction was kept warm for 3 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced to obtain 15.6 g of epoxidized amide;
[0088] 13.0 g of epoxidized amide, 5.0 g of 2,6,10-trimethyl-2,6,10-pentadecatriene-14-one, 5.0 g of (2E, 4E)-5-(4-methoxy-2,3,6-trimethylphenyl)-3-methyl-2,4-pentadienal, 2.4 g of γ-alumina and 40.0 g of dimethyl sulfoxide were weighed and added into a reactor. The temperature of the reactor was raised to 80°C and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction solution was added into a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 22.4 g of extended chain fatty acid amide.
[0089] S2. Preparation of epoxidized amide
[0090] 21.0 g of chain-extended fatty acid amide, 8.0 g of 2,3-biphenyl maleic anhydride, 85.0 g of dimethyl sulfoxide and 2.4 g of aluminum chloride were weighed and added to a reactor. The temperature of the reactor was raised to 170° C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100° C., and distilled under reduced pressure until no liquid was produced, to obtain 28.3 g of acidified polyamide;
[0091] 3.0 g of N-hydroxysuccinimide, 1.5 g of N,N-dicyclohexylcarbodiimide, 0.4 g of triethylamine and 36.0 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 1 hour, 20.0 g of acidified polyamide was added to the reactor. The temperature of the reactor was raised to 50° C. and the reaction was kept warm for 4 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced to obtain 22.1 g of imidized polyamide;
[0092] 20.0 g of imidized polyamide, 3.6 g of glacial acetic acid, 2.4 g of hydrogen peroxide and 72.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 80°C and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 21.0 g of epoxidized amide.
[0093] S3. Preparation of silicon nitride oil
[0094] Weigh 6.0 g of methyl high hydrogen silicone oil, 1.5 g of ammonium fluoride, 0.4 g of silver fluoride and 13.4 g of benzene into a reactor and react at room temperature for 6 h. After the reactor is cooled to room temperature, the reaction solution is added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid is produced to obtain 6.2 g of fluorinated silicone oil;
[0095] 5.4 g of fluorinated silicone oil, 3.3 g of tetramethyldivinyldisiloxane, 15.4 g of 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane and 33.4 g of ether were weighed and added into a reaction kettle, and stirred at room temperature for 20 min to obtain 57.5 g of reaction precursor solution;
[0096] Weigh 56.0 g of the reaction precursor solution and 5.6 g of 98 wt % sulfuric acid solution into a reactor, keep the reaction at room temperature for 10 h to obtain a reaction solution, add solid sodium bicarbonate to the reaction solution until the pH of the reaction solution is 8, cool the reactor to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 100° C., and distill under reduced pressure until no liquid is produced to obtain telomerized silicone oil;
[0097] 20.0 g of polysilicone oil, 8.0 g of triaminosilane, 1.0 g of chloroplatinic acid and 50.0 g of xylene were weighed and added to a reactor. The temperature of the reactor was raised to 60°C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 27.5 g of ammoniated silicone oil.
[0098] S4. Preparation of lubricant
[0099] 18.0 g of epoxidized amide and 24.0 g of aminated silicone oil were added into a reaction kettle and stirred evenly to obtain a lubricant for polyvinyl chloride.
[0100] Example 3
[0101] This embodiment provides a method for preparing an environmentally friendly and efficient lubricant for polyvinyl chloride, comprising the following steps:
[0102] S1. Preparation of chain-extended fatty acid amide
[0103] Weigh 18.7 g of 8,13-dimethyl-8,12-eicosenedioic acid, 5.4 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, and 54.0 g of dimethyl sulfoxide into a reactor, stir at room temperature for 8 min, drop the reactor temperature to 3°C, add 0.8 g of 1-hydroxybenzotriazole and 0.8 g of dicyclohexylcarbodiimide, and keep the reaction for 2 h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 90°C, and distill under reduced pressure until no liquid is produced to obtain 21.6 g of modified fatty acid amide;
[0104] 20.0 g of modified fatty acid amide, 4.8 g of glacial acetic acid, 3.2 g of hydrogen peroxide and 54.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 70°C and kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90°C and distilled under reduced pressure until no liquid was produced to obtain 21.6 g of epoxidized amide;
[0105] 18.0 g of epoxidized amide, 6.7 g of 2,6,10-trimethyl-2,6,10-pentadecatriene-14-one, 6.7 g of (2E, 4E)-5-(4-methoxy-2,3,6-trimethylphenyl)-3-methyl-2,4-pentadienal, 3.2 g of γ-alumina and 50.0 g of dimethyl sulfoxide were weighed and added into a reactor. The temperature of the reactor was raised to 70°C and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction solution was added into a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was produced to obtain 31.2 g of extended chain fatty acid amide.
[0106] S2. Preparation of epoxidized amide
[0107] 28.0 g of chain-extended fatty acid amide, 10.7 g of 2,3-biphenyl maleic anhydride, 106.7 g of dimethyl sulfoxide and 2.6 g of aluminum chloride were weighed and added to a reactor. The temperature of the reactor was raised to 160° C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 90° C., and distilled under reduced pressure until no liquid was produced, to obtain 36.4 g of acidified polyamide;
[0108] 4.7 g of N-hydroxysuccinimide, 2.0 g of N,N-dicyclohexylcarbodiimide, 0.67 g of triethylamine and 42.7 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 1 hour, 26.7 g of acidified polyamide was added to the reactor. The temperature of the reactor was raised to 45° C. and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced to obtain 30.8 g of imidized polyamide;
[0109] 26.7 g of imidized polyamide, 5.4 g of glacial acetic acid, 3.3 g of hydrogen peroxide and 100.0 g of N,N-dimethylformamide were weighed and added into a reactor. The temperature of the reactor was raised to 70°C and kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was extracted to obtain epoxidized amide.
[0110] S3. Preparation of silicon nitride oil
[0111] Weigh 6.7 g of methyl high hydrogen silicone oil, 1.3 g of ammonium fluoride, 0.4 g of silver fluoride and 14.4 g of benzene into a reactor and react at room temperature for 5 h. After the reactor is cooled to room temperature, the reaction solution is added to a rotary evaporator with a water bath temperature of 90°C and distilled under reduced pressure until no liquid is produced to obtain 7.2 g of fluorinated silicone oil;
[0112] 6.7 g of fluorinated silicone oil, 3.3 g of tetramethyldivinyldisiloxane, 14.0 g of 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane and 33.3 g of ether were weighed and added into a reaction kettle, and stirred at room temperature for 20 min to obtain 44.3 g of reaction precursor solution;
[0113] Weigh 44.3 g of the reaction precursor solution and 4.4 g of 98 wt % sulfuric acid solution into a reactor, and keep the reaction at room temperature for 9 h to obtain a reaction solution. Add solid sodium bicarbonate to the reaction solution until the pH of the reaction solution is 8. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 90° C., and distill under reduced pressure until no liquid is produced to obtain 22.3 g of telomerized silicone oil;
[0114] 21.0 g of polysilicone oil, 7.0 g of triaminosilane, 1.0 g of chloroplatinic acid and 42.0 g of xylene were weighed and added to a reactor. The temperature of the reactor was raised to 55°C. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 27.5 g of ammoniated silicone oil.
[0115] S4. Preparation of lubricant
[0116] 24.0 g of epoxidized amide and 24.0 g of aminated silicone oil were added into a reaction kettle and stirred evenly to obtain a lubricant for polyvinyl chloride.
[0117] Comparative Example 1
[0118] The difference between this comparative example and Example 3 is that step S1 and step S2 are eliminated, and in step S4, an equal amount of polyethylene wax is used to replace epoxidized amide.
[0119] Comparative Example 2
[0120] The difference between this comparative example and Example 3 is that step S3 is eliminated, and in step S4, methyl high hydrogen silicone oil is used instead of silicon nitride oil.
[0121] Comparative Example 3
[0122] The difference between this comparative example and Example 3 is that step S3 is eliminated, and in step S4, the use of silicon nitride oil is eliminated.
[0123] Performance Testing:
[0124] A mixture was formed by using the lubricant, polyvinyl chloride and auxiliary materials prepared in Examples 1-3 and Comparative Examples 1-3, respectively, and added into a twin-screw extruder. The temperatures of the eight temperature sections of the twin-screw extruder from the feed port to the discharge port were 160°C, 165, 165°C, 170°C, 170°C, 180°C and 180°C, respectively. The main engine speed of the twin-screw extruder was 100 rpm and the pressure was 125 bar. A plastic hose sample with a thickness of 160 mm was obtained by melt extrusion. The plastic hose sample was used as a test piece. The release of acidic gas during the preparation of the plastic hose sample was determined by referring to the standard GB / T2917.1-2002 "Determination of hydrogen chloride and any other acidic products released by blends and products based on vinyl chloride homopolymers and copolymers at high temperatures - Congo red method". The test results are shown in Table 1.
[0125] 1. For the wear resistance of plastic hose samples, refer to QB / T 5101-2017 "Test method for wear resistance of plastic hoses". Place the plastic hose sample in a device filled with abrasive media and swing it 100,000 times to measure the mass loss.
[0126] 2. The tensile strength of the plastic hose specimens is measured with reference to the standard GB / T 8804.1-2003 "Determination of tensile properties of thermoplastic plastic pipes Part 1: General principles of test methods" to measure the elongation at break of the plastic hose specimens.
[0127] 3. The surface smoothness of the plastic hose sample is tested according to the standard GB / T 10006-2021 "Determination of the friction coefficient of plastic films and sheets".
[0128] 4. The plastic hose samples were treated at 200°C for 1 hour to test their softness and the plastic hose samples were treated at 120°C for 36 days to test their cracking. The specific results are shown in Table 2.
[0129] Table 1-Statistics of Congo red test paper color change time during sample preparation
[0130]
[0131] Table 2-Test data table of each test sample
[0132]
[0133] Data Analysis:
[0134] Comparative analysis was performed on the data in Table 1 above. The plastic hose sample prepared using the lubricant for polyvinyl chloride prepared by the present invention was shaken 100,000 times in an apparatus equipped with abrasive media, and the mass loss was 6.0 g. After high-temperature treatment at 200° C. for 1 hour, the plastic hose could be wound 7 times. After heat preservation at 120° C. for 36 days, the plastic hose did not crack. The surface friction coefficient of the plastic hose was only 0.295, the elongation at break was 193%, and the color change time of the Congo red test paper during the preparation process was 965 s.
[0135] All data are better than those of the comparative example, indicating that in this experiment, after preparing a long-chain fatty acid amide, the epoxy amide is epoxidized, chain extended, acidified, imidized and subjected to secondary epoxidation, and the nitrided silicone oil obtained by fluorinating the p-methyl high hydrogen silicone oil of the present invention and then nitriding it with a siloxane organic matter, in the lubricant for polyvinyl chloride obtained by mixing, the abundant epoxy groups inside the epoxy amide combine with the hydrogen chloride gas generated after the pyrolysis of polyvinyl chloride to reduce environmental pollution, while enhancing the complexity of the polyvinyl chloride chain segment, and through the reaction, a ring structure is added to the polyvinyl chloride chain segment, thereby enhancing its tensile strength and wear resistance;
[0136] The rich high-temperature resistant groups inside the two, such as fluorine groups and imide groups, further enhance the high-temperature resistance of the polyvinyl chloride material after molding. Silicone nitride oil reduces the polarity of the polyvinyl chloride chain segment and enhances its compatibility with auxiliary materials. While reducing its surface friction coefficient and improving its surface smoothness, it indirectly participates in the improvement of its various functions.
[0137] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0138] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0139] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An environmentally friendly and efficient lubricant for polyvinyl chloride, It is characterized in that The method comprises the following raw material components in parts by weight: 10-20 parts of epoxidized amide and 15-40 parts of aminated silicone oil; The preparation method of epoxidized amide is as follows: 20-25 parts of imidized polyamide, 3-5 parts of glacial acetic acid, 2-4 parts of hydrogen peroxide and 60-80 parts of N,N-dimethylformamide are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the epoxidized amide is obtained by post-treatment.
2. An environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 1, It is characterized in that The preparation method of the imidized polyamide is as follows: 3-5 parts of N-hydroxysuccinimide, 1-2 parts of N,N-dicyclohexylcarbodiimide, 0.3-0.5 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, reacted at room temperature for 0.5-1h, 20-30 parts of acidified polyamide are added into the reaction kettle, the temperature of the reaction kettle is increased to 40-50°C, the reaction is kept warm for 2-4h, and the imidized polyamide is obtained by post-treatment.
3. An environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 2, It is characterized in that The preparation method of the acidified polyamide is as follows: 20-30 parts of chain-extended fatty acid amide, 5-10 parts of 2,3-biphenyl maleic anhydride, 75-100 parts of dimethyl sulfoxide and 1-3 parts of aluminum chloride are weighed and added into a reactor, the temperature of the reactor is raised to 150-170° C., and the acidified polyamide is obtained by post-treatment.
4. An environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 3, It is characterized in that The preparation method of the chain-extended fatty acid amide is as follows: 10-15 parts of epoxidized amide, 5-8 parts of 2,6,10-trimethyl-2,6,10-pentadecatriene-14-one, 5-8 parts of (2E,4E)-5-(4-methoxy-2,3,6-trimethylphenyl)-3-methyl-2,4-pentadienal, 2-3 parts of γ-alumina and 30-40 parts of dimethyl sulfoxide are weighed by weight and added into a reaction kettle, the temperature of the reaction kettle is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the chain-extended fatty acid amide is obtained by post-treatment.
5. An environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 4, It is characterized in that The preparation method of epoxidized amide is as follows: 10-15 parts of modified fatty acid amide, 3-5 parts of glacial acetic acid, 2-4 parts of hydrogen peroxide and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, the temperature of the reaction kettle is increased to 60-80°C, the reaction is kept warm for 2-3 hours, and the epoxidized amide is obtained by post-treatment.
6. The environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 5, It is characterized in that The preparation method of the modified fatty acid amide is as follows: 20-30 parts of 8,13-dimethyl-8,12-eicosenedioic acid, 5-10 parts of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether and 75-100 parts of dimethyl sulfoxide are weighed by weight and added into a reaction kettle, stirred at room temperature for 5-10 minutes, the temperature of the reaction kettle is lowered to 0-5°C, 1-2 parts of 1-hydroxybenzotriazole and 1-2 parts of dicyclohexylcarbodiimide are added thereto, the reaction is kept warm for 1-2 hours, and the modified fatty acid amide is obtained by post-treatment.
7. The environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 1, It is characterized in that The preparation method of ammoniated silicone oil is as follows: 20-30 parts of modified silicone oil, 6-8 parts of triaminosilane, 0.5-1.5 parts of chloroplatinic acid and 40-50 parts of xylene are weighed and added into a reactor, the temperature of the reactor is increased to 50-60° C., and the ammoniated silicone oil is obtained by post-treatment.
8. An environmentally friendly and efficient lubricant for polyvinyl chloride according to claim 7, It is characterized in that The preparation method of telomerized silicone oil comprises the following steps: A1, weigh 20-30 parts of methyl high hydrogen silicone oil, 3-5 parts of ammonium fluoride, 0.5-1.5 parts of silver fluoride and 40-50 parts of benzene by weight, add them into a reaction kettle, react at room temperature for 4-6 hours, and post-treat to obtain fluorinated silicone oil; A2, weigh 8-10 parts of fluorinated silicone oil, 3-5 parts of tetramethyldivinyldisiloxane, 20-25 parts of 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane and 40-50 parts of ether by weight, add them into a reaction kettle, and stir at room temperature for 15-20 minutes to obtain a reaction precursor solution; A3, weighing 20-30 parts of reaction precursor solution and 2-3 parts of 98wt% sulfuric acid solution by weight, adding them into the reaction kettle, keeping the temperature at room temperature for 8-10 hours to obtain a reaction solution; A4. Add solid sodium bicarbonate to the reaction kettle containing the reaction solution until the pH of the reaction solution is 7-8, and then perform post-treatment to obtain telomerized silicone oil.
9. A method for preparing an environmentally friendly and efficient lubricant for polyvinyl chloride according to any one of claims 1 to 8, It is characterized in that The specific preparation method is to add epoxidized amide and ammoniated silicone oil into a reaction kettle and stir evenly to obtain an environmentally friendly and efficient lubricant for polyvinyl chloride.
Citation Information
Cited By
Precipitation-free lubricant and preparation method thereof
CN120365488A