Heat-conducting gasket, preparation method thereof and optical module

Thermal gaskets are prepared by high-temperature vacuum extraction and self-crosslinking reaction, which solves the problems of high volatility and oil output in the thermal management of optical modules, and realizes low-cost, low-volatility and high-stability thermal gaskets. Improves the reliability and durability of the equipment.

CN118994915APending Publication Date: 2024-11-22SHENZHEN HFC SHIELDING PRODS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411090710.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The thermal management difficulties arising from optical modules under high transmission rates and data processing requirements, the volatility and oil output of existing thermal gaskets affect equipment stability and reliability.

Method used

Thermal gasket is prepared by high-temperature vacuum treatment and self-crosslinking reaction. The volatile substances are removed by drying and stirring, forming a network structure, avoiding the addition of additional catalysts and inhibitors, and reducing volatility and oil output.

Benefits of technology

Thermal gasket with low volatility and oil output is obtained, which improves the stability and durability of the equipment, reduces the potential impact on the optical components inside the optical module, and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986478350000141
    Figure BDA0004986478350000141
Patent Text Reader

Abstract

The invention provides a heat-conducting gasket, a preparation method thereof and an optical module, and belongs to the technical field of electronic materials. The preparation method of the heat-conducting gasket comprises the following steps: vacuumizing raw materials containing hydrogen-containing silicone oil, vinyl silicone oil and heat-conducting powder to obtain a first mixture, then calendering the first mixture to obtain a calendered sheet, and curing the calendered sheet at the temperature of 150-200 DEG C for 2-6 hours to obtain the heat-conducting gasket. According to the preparation method, volatile substances in the raw materials can be removed through vacuumizing treatment in a high-temperature state, then the hydrogen-containing silicone oil and the vinyl silicone oil form a network structure through the self-crosslinking reaction in the high-temperature state, so that the network structure is cured to form the heat-conducting gasket, and the self-crosslinking reaction does not need to additionally add a platinum catalyst and an inhibitor; and the self-crosslinking reaction is carried out in a high-temperature state, and the volatile matters in the calendered sheet can be discharged again at a high temperature, so that the volatility of the prepared heat-conducting gasket is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electronic materials, and in particular to a thermally conductive gasket and a preparation method thereof, and an optical module. Background Art

[0002] As the core device in the optical fiber communication system, the performance of the optical module directly affects the quality and efficiency of communication. With the rapid development of 5G networks and the large-scale construction of data centers, the transmission rate and data processing capabilities of optical modules are increasingly required, which leads to an increase in the heat generated by the optical module during operation. Therefore, an effective thermal management solution is essential to ensure the stability of the optical module and extend its service life.

[0003] Low volatility and low oil output thermal pads are mainly used for heat dissipation of electronic equipment, especially in environments that require low oil output and low volatility. For example, it can be used for heat transfer between a heat sink or base and an IC power device, effectively reducing contact thermal resistance and improving heat dissipation efficiency. In addition, due to its low volatility, thermal pads are also very suitable for heat dissipation applications in high-performance filters, optical cameras or LED lights, which can avoid the generation of condensation or mist, and low oil output thermal pads can reduce the failure rate caused by silicone oil penetration and improve the stability and reliability of the equipment. Summary of the invention

[0004] The present application provides a thermally conductive gasket and a preparation method thereof, and an optical module, which have low volatility and low oil yield.

[0005] The embodiment of the present application is implemented as follows:

[0006] In the first aspect, the example of the present application provides a method for preparing a thermally conductive gasket, which includes first subjecting a raw material containing hydrogenated silicone oil, vinyl silicone oil and thermally conductive powder to a vacuum treatment to obtain a first mixture, then subjecting the first mixture to a calendering treatment to a calendered sheet, and curing the calendered sheet at a temperature of 150°C to 200°C for 2h to 6h to obtain a thermally conductive gasket; the vacuum treatment includes vacuuming at a temperature of 125°C to 150°C for 1h to 4h.

[0007] In the above technical scheme, the preparation method of the thermally conductive gasket of the present application first performs a vacuum treatment under a high temperature state to remove volatile substances in the raw materials, and then uses a self-crosslinking reaction under a high temperature state to allow hydrogen-containing silicone oil and vinyl silicone oil to form a network structure to solidify and form a thermally conductive gasket. The self-crosslinking reaction not only does not require the additional addition of platinum catalysts and inhibitors, thereby avoiding the introduction of volatiles and reducing costs, but also the self-crosslinking reaction is carried out under a high temperature state, and the calendered sheet can discharge the volatiles therein again at a high temperature, thereby reducing the volatility of the obtained thermally conductive gasket; at the same time, the self-crosslinking reaction avoids the generation of excess free silicone oil, reduces the oil yield of the obtained thermally conductive gasket, and thereby obtains a thermally conductive gasket with a lower oil yield, thereby reducing the potential impact of volatiles and oily substances in the thermally conductive gasket on the optical elements inside the optical module, and the thermally conductive gasket has good stability and durability.

[0008] In combination with the first aspect, in a first possible example of the first aspect of the present application, a stirring state is maintained during the vacuum treatment.

[0009] In the above example, maintaining a stirring state during the vacuuming process can make the vacuuming more uniform, thereby more thoroughly removing the volatile substances in the raw materials and reducing the volatility of the obtained thermally conductive gasket.

[0010] In combination with the first aspect, in a second possible example of the first aspect of the present application, before the vacuum treatment, the raw material is dried at 125° C. to 150° C. for 1 h to 4 h.

[0011] In the above example, the raw materials are dried at the above temperature and for the above time before vacuum treatment. On the one hand, this can prevent the raw materials from undergoing cross-linking reaction and thus solidification. On the other hand, the drying treatment can remove volatile substances in the raw materials and reduce the volatility of the resulting thermally conductive gasket.

[0012] In combination with the first aspect, in a third possible example of the first aspect of the present application, the raw materials include 1wt% to 20wt% hydrogenated silicone oil, 1wt% to 10wt% vinyl silicone oil and 70wt% to 90wt% thermal conductive powder.

[0013] In combination with the first aspect, in a fourth possible example of the first aspect of the present application, the viscosity of the hydrogen-containing silicone oil is 20 mPa·s to 100 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.01% to 1%.

[0014] In the above example, by making the viscosity of the hydrogenated silicone oil within the above range, the thermally conductive gasket can be filled with more thermally conductive powder, thereby achieving a better thermal conductive effect.

[0015] In combination with the first aspect, in a fifth possible example of the first aspect of the present application, the viscosity of the vinyl silicone oil is 100 mPa·s to 500 mPa·s, and the vinyl content of the vinyl silicone oil is 0.1% to 1%.

[0016] In the above example, by making the viscosity of the vinyl silicone oil within the above range, the thermally conductive gasket can be filled with more thermally conductive powder, thereby having a better thermal conductive effect.

[0017] In combination with the first aspect, in a sixth possible example of the first aspect of the present application, the above-mentioned thermal conductive powder includes any one or more of aluminum oxide powder, zinc oxide powder, boron nitride powder, aluminum nitride powder, aluminum powder, silver powder, diamond powder, graphite, graphene and carbon nanotubes.

[0018] In the above example, the thermally conductive powder can be used to fill the network structure formed by hydrogenated silicone oil and vinyl silicone oil to improve the thermal conductivity of the thermally conductive gasket.

[0019] In combination with the first aspect, in the seventh possible example of the first aspect of the present application, the above-mentioned raw materials also include 0.1wt% to 3wt% of auxiliary agents, and the auxiliary agents include any one or more of high temperature resistant auxiliary agents, viscosity enhancers, antioxidants and anti-aging agents.

[0020] In a second aspect, the present application example provides a thermally conductive gasket, which is manufactured according to the above-mentioned method for manufacturing a thermally conductive gasket.

[0021] In the above technical solution, the thermally conductive gasket of the present application has lower volatility and oil yield.

[0022] In a third aspect, the present application example provides an optical module, which includes the above-mentioned thermal conductive gasket. DETAILED DESCRIPTION

[0023] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0024] The following is a detailed description of a thermally conductive gasket and a preparation method thereof, and an optical module according to an embodiment of the present application:

[0025] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:

[0026] S1. Drying

[0027] Dry the raw material at 125°C to 150°C for 1 h to 4 h.

[0028] As an example, the drying temperature of the raw material may be 125°C, 130°C, 135°C, 140°C, 145°C or 150°C; the drying time of the raw material may be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.

[0029] The raw materials include 1wt% to 20wt% of hydrogen-containing silicone oil, 1wt% to 10wt% of vinyl silicone oil and 70wt% to 90wt% of thermal conductive powder.

[0030] The viscosity of the hydrogen-containing silicone oil is 20 mPa·s to 100 mPa·s.

[0031] As an example, the viscosity of the hydrogen-containing silicone oil can be 20mPa·s, 25mPa·s, 30mPa·s, 35mPa·s, 40mPa·s, 45mPa·s, 50mPa·s, 55mPa·s, 60mPa·s, 65mPa·s, 70mPa·s, 75mPa·s, 80mPa·s, 85mPa·s, 90mPa·s, 95mPa·s or 100mPa·s.

[0032] By making the viscosity of the hydrogen-containing silicone oil within the above range, the thermally conductive gasket can be filled with more thermally conductive powder, thereby achieving a better thermal conductive effect.

[0033] The hydrogen content of hydrogen-containing silicone oil is 0.01% to 1%.

[0034] It should be noted that the hydrogen content of the hydrogen-containing silicone oil refers to the content of hydrogen atoms.

[0035] As an example, the hydrogen content of the hydrogen-containing silicone oil may be 0.01%, 0.02%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%.

[0036] The viscosity of vinyl silicone oil is 100 mPa·s to 500 mPa·s.

[0037] As an example, the viscosity of the vinyl silicone oil may be 100 mPa·s, 150 mPa·s, 200 mPa·s, 250 mPa·s, 300 mPa·s, 350 mPa·s, 400 mPa·s, 450 mPa·s, or 500 mPa·s.

[0038] By making the viscosity of the vinyl silicone oil within the above range, the thermally conductive gasket can be filled with more thermally conductive powder, thereby achieving a better thermal conductive effect.

[0039] The vinyl content of vinyl silicone oil is 0.1% to 1%.

[0040] It should be noted that the vinyl content of the vinyl silicone oil refers to the content of vinyl groups.

[0041] As an example, the vinyl content of the vinyl silicone oil may be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%.

[0042] The thermally conductive powder includes any one or more of aluminum oxide powder, zinc oxide powder, boron nitride powder, aluminum nitride powder, aluminum powder, silver powder, diamond powder, graphite, graphene and carbon nanotubes.

[0043] As an example, the thermally conductive powder may be a single aluminum oxide powder, zinc oxide powder, boron nitride powder, aluminum nitride powder, aluminum powder, silver powder, diamond powder, graphite, graphene or carbon nanotubes, or may be a mixture of aluminum oxide powder and zinc oxide powder, or may be a mixture of aluminum powder and silver powder, or may be a mixture of graphene and carbon nanotubes, or may be a mixture of aluminum oxide powder and aluminum nitride powder, or may be a mixture of zinc oxide powder and boron nitride powder, or may be a mixture of aluminum oxide powder, zinc oxide powder, boron nitride powder and aluminum nitride powder, or may be a mixture of boron nitride powder, aluminum nitride powder, aluminum powder, silver powder and diamond powder, or may be a mixture of graphite, graphene and carbon nanotubes.

[0044] The thermally conductive powder can be used to fill the network structure formed by hydrogenated silicone oil and vinyl silicone oil to improve the thermal conductivity of the thermally conductive gasket.

[0045] The raw material also includes 0.1wt% to 3wt% of an auxiliary agent, and the auxiliary agent includes any one or more of a high temperature resistant auxiliary agent, a tackifier, an antioxidant and an anti-aging agent.

[0046] The high temperature resistant additive includes any one or more of potassium titanate whisker, magnesium oxide, zinc oxide, montmorillonite additive and rare earth heat resistant agent.

[0047] The tackifier includes any one or more of fumed silica, hydrogenated castor oil, polyamide wax and polyethylene micropowder.

[0048] The antioxidant includes any one or more of phenolic antioxidants, n-octadecyl propionate and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0049] Anti-aging agents include cerium oxide and / or iron oxide.

[0050] It should be noted that the drying treatment of the raw materials may be performed by mixing the raw materials according to the proportion and then drying the mixture at the above temperature and for the above time, or by drying the raw materials separately at the above temperature and for the above time.

[0051] Drying the raw materials at the above temperature and for the above time can, on the one hand, prevent the raw materials from undergoing a cross-linking reaction and thereby solidifying, and on the other hand, can remove volatile substances in the raw materials through the drying process, thereby reducing the volatility of the resulting thermally conductive gasket.

[0052] S2. Vacuum treatment

[0053] After the raw materials are mixed, vacuum treatment is performed to obtain a first mixture, and the vacuum treatment includes vacuuming at a temperature of 125° C. to 150° C. for 1 hour to 4 hours.

[0054] As an example, the temperature of vacuum drying can be 125°C, 130°C, 135°C, 140°C, 145°C or 150°C; the time of vacuum treatment can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.

[0055] In some embodiments, the vacuum degree of the vacuum treatment is ≤0.09 MPa.

[0056] In some embodiments, stirring is maintained during the vacuum process.

[0057] Maintaining a stirring state during the vacuuming process can make the vacuuming more uniform, thereby more thoroughly removing the volatile substances in the raw materials and reducing the volatility of the obtained thermally conductive gasket.

[0058] Optionally, a stirring state with a stirring rate of 20 rpm to 50 rpm is maintained during the vacuum treatment.

[0059] S3. Preparation of thermal conductive pads

[0060] The first mixture is subjected to calendering treatment to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 150° C. to 200° C. for 2 hours to 6 hours to obtain a thermally conductive pad.

[0061] As an example, the temperature of the curing reaction can be 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C; the time of the curing reaction can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0062] The preparation method of the thermally conductive gasket of the present application first performs a vacuum treatment under a high temperature state to remove volatile substances in the raw materials, and then uses a self-crosslinking reaction under a high temperature state to allow hydrogen-containing silicone oil and vinyl silicone oil to form a network structure to solidify and form a thermally conductive gasket. The self-crosslinking reaction not only does not require the additional addition of platinum catalysts and inhibitors, thereby avoiding the introduction of volatiles and reducing costs, but the self-crosslinking reaction is carried out under a high temperature state, and the calendered sheet can discharge the volatiles therein again at a high temperature, thereby reducing the volatility of the thermally conductive gasket obtained; at the same time, the self-crosslinking reaction avoids the generation of excess free silicone oil, reduces the oil yield of the thermally conductive gasket obtained, and thereby obtains a thermally conductive gasket with a lower oil yield, reduces the potential impact of volatiles and oily substances in the thermally conductive gasket on the optical elements inside the optical module, and the thermally conductive gasket has good stability and durability.

[0063] The present application also provides a thermally conductive gasket, which is prepared according to the above-mentioned method for preparing the thermally conductive gasket.

[0064] The thermally conductive pad of the present application has lower volatility and oil yield.

[0065] The present application also provides an optical module, which includes the above-mentioned thermal conductive gasket.

[0066] The following is a further detailed description of a thermally conductive gasket and a preparation method thereof of the present application in conjunction with embodiments.

[0067] Example 1

[0068] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0069] S1. Drying

[0070] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0071] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0072] S2. Vacuum treatment

[0073] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0074] S3. Preparation of thermal conductive pads

[0075] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0076] Example 2

[0077] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0078] S1. Drying

[0079] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0080] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0081] S2. Vacuum treatment

[0082] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0083] S3. Preparation of thermal conductive pads

[0084] The first mixture is calendered by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 150° C. for 6 hours to obtain a thermally conductive gasket.

[0085] Example 3

[0086] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0087] S1. Drying

[0088] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0089] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0090] S2. Vacuum treatment

[0091] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0092] S3. Preparation of thermal conductive pads

[0093] The first mixture is calendered by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 180° C. for 2 hours to obtain a thermally conductive gasket.

[0094] Example 4

[0095] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0096] S1. Drying

[0097] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0098] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0099] S2. Vacuum treatment

[0100] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 125°C and the vacuum was evacuated for 6 hours to obtain the first mixture.

[0101] S3. Preparation of thermal conductive pads

[0102] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0103] Example 5

[0104] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0105] S1. Drying

[0106] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 125° C. for 4 h, respectively.

[0107] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0108] S2. Vacuum treatment

[0109] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0110] S3. Preparation of thermal conductive pads

[0111] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0112] Example 6

[0113] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0114] S1. Drying

[0115] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 140° C. for 2 h, respectively.

[0116] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0117] S2. Vacuum treatment

[0118] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0119] S3. Preparation of thermal conductive pads

[0120] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0121] Example 7

[0122] The present invention provides a thermally conductive pad and a method for preparing the same, which comprises the following steps:

[0123] S1. Drying

[0124] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 92 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0125] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0126] S2. Vacuum treatment

[0127] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0128] S3. Preparation of thermal conductive pads

[0129] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0130] Comparative Example 1

[0131] The comparative example of the present application provides a thermally conductive pad and a preparation method thereof, which comprises the following steps:

[0132] S1. Drying

[0133] 10 g of vinyl silicone oil, 2 g of hydrogen-containing silicone oil and 90 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively, and cooled to room temperature.

[0134] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0135] S2. Vacuum treatment

[0136] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide, 1 g of antioxidant 1010, 0.5 g of platinum catalyst and 0.015 g of inhibitor were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at a temperature of 25°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0137] S3. Preparation of thermal conductive pads

[0138] The first mixture is subjected to calendering treatment by a calendering machine to obtain a thermally conductive pad.

[0139] Comparative Example 2

[0140] The comparative example of the present application provides a thermally conductive pad and a preparation method thereof, which comprises the following steps:

[0141] S1. Drying

[0142] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0143] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0144] S2. Vacuum treatment

[0145] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0146] S3. Preparation of thermal conductive pads

[0147] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 1 hour to obtain a thermally conductive gasket.

[0148] Comparative Example 3

[0149] The comparative example of the present application provides a thermally conductive pad and a preparation method thereof, which comprises the following steps:

[0150] S1. Drying

[0151] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0152] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0153] S2. Vacuum treatment

[0154] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 150°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0155] S3. Preparation of thermal conductive pads

[0156] The first mixture was calendered by a calendering machine to obtain a calendered sheet, and the calendered sheet was cured at a temperature of 140° C. for 4 hours to obtain a thermally conductive gasket.

[0157] Comparative Example 4

[0158] The comparative example of the present application provides a thermally conductive pad and a preparation method thereof, which comprises the following steps:

[0159] S1. Drying

[0160] 1 g of vinyl silicone oil, 15 g of hydrogen-containing silicone oil and 86 g of alumina powder were weighed, and the vinyl silicone oil, hydrogen-containing silicone oil and alumina powder were dried at 150° C. for 1 h, respectively.

[0161] The viscosity of the vinyl silicone oil is 450 mPa·s, and the vinyl content of the vinyl silicone oil is 0.4%; the viscosity of the hydrogen-containing silicone oil is 50 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.8%.

[0162] S2. Vacuum treatment

[0163] The dried vinyl silicone oil, hydrogenated silicone oil and alumina powder were added to the stirring kettle in turn, and then 6 g of iron oxide and 1 g of antioxidant 1010 were added to the stirring kettle. The rotation speed was set to 25 rpm and the vacuum degree was set to 0.09 MPa. The stirring state was maintained at 100°C and the vacuum was evacuated for 1 hour to obtain the first mixture.

[0164] S3. Preparation of thermal conductive pads

[0165] The first mixture is subjected to calendering treatment by a calendering machine to obtain a calendered sheet, and the calendered sheet is cured at a temperature of 200° C. for 4 hours to obtain a thermally conductive gasket.

[0166] Test Example 1

[0167] The thermally conductive gaskets prepared in Examples 1 to 7 and Comparative Examples 1 to 4 were taken to measure their thermal conductivity, hardness, condensable volatility, presence or absence of condensate, D3-D20 content and oil yield. The results are shown in Table 1.

[0168] The test method is as follows:

[0169] 1. Thermal conductivity

[0170] The test was performed according to ASTM D5470.

[0171] 2. Hardness

[0172] The test was carried out according to ASTM D 2240.

[0173] 3. Condensable volatility

[0174] The test was performed according to ASTM E595.

[0175] 4. Whether there is condensation

[0176] Place 10g of thermally conductive pad into a 500ml volumetric flask, cover the flask with a glass lid, place the volumetric flask on a 150℃ baking table, and observe whether there is any volatile condensate on the glass after 48 hours.

[0177] 5. D3-D20 content

[0178] The test was performed according to the method of ASTM F2466.

[0179] 6. Oil yield

[0180] There are 4 layers of filter paper and 4 layers of glass fiber cloth on the top and bottom. The sample is sandwiched in the middle. A stainless steel gasket with 50% compression of the sample is placed on the fixture nut and tightened. The sample is placed in a 125℃ constant temperature oven for 48 hours.

[0181] Table 1 Parameters of thermally conductive pads obtained in Examples 1 to 7 and Comparative Examples 1 to 4

[0182]

[0183] It can be seen from Examples 1 to 7 of the present application that the thermally conductive gasket prepared by the preparation method of the thermally conductive gasket of the present application has a relatively high thermal conductivity, a condensable volatility of ≤0.032%, no condensate, and a D3-D20 content of ≤42 ppm.

[0184] From the comparison between Comparative Example 1 and Example 1, it can be seen that Comparative Example 1 is cured by adding a platinum catalyst system, and the condensable volatility of the obtained thermal conductive gasket is as high as 0.076%, there is condensate, and the D3-D20 content is as high as 83 ppm.

[0185] By comparing Comparative Example 2 with Example 1, it can be seen that the curing time of Comparative Example 2 is only 1 hour, the self-crosslinking reaction of hydrogenated silicone oil and vinyl silicone oil has not been completely completed, the condensable volatility of the prepared thermal conductive gasket is as high as 0.039%, there is condensate, and the D3-D20 content is as high as 49ppm.

[0186] By comparing Comparative Example 3 and Example 1, it can be seen that the curing temperature of Comparative Example 3 is 150°C, the self-crosslinking reaction of hydrogenated silicone oil and vinyl silicone oil has not been completely completed, the condensable volatility of the prepared thermal conductive gasket is as high as 0.035%, there is condensate, and the D3-D20 content is as high as 46ppm.

[0187] By comparing Comparative Example 4 with Example 1, it can be seen that the vacuum temperature of Comparative Example 4 is only 100°C, the volatile substances in the raw materials are not completely removed, the condensable volatility of the prepared thermal conductive gasket is as high as 0.036%, there is condensate, and the D3-D20 content is as high as 48ppm.

[0188] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a thermally conductive gasket, characterized in that: The preparation method of the thermally conductive gasket comprises: firstly subjecting raw materials including hydrogenated silicone oil, vinyl silicone oil and thermally conductive powder to a vacuum treatment to obtain a first mixture, then subjecting the first mixture to a calendering treatment to obtain a calendered sheet, and curing the calendered sheet at a temperature of 150° C. to 200° C. for 2 h to 6 h to obtain a thermally conductive gasket; The vacuum treatment includes vacuuming at a temperature of 125° C. to 150° C. for 1 hour to 4 hours.

2. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The stirring state is maintained during the vacuum treatment.

3. The method for preparing a thermally conductive pad according to claim 1, characterized in that: Before the vacuum treatment, the raw material is dried at 125° C. to 150° C. for 1 h to 4 h.

4. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The raw materials include 1wt% to 20wt% of the hydrogen-containing silicone oil, 1wt% to 10wt% of the vinyl silicone oil and 70wt% to 90wt% of the thermal conductive powder.

5. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The viscosity of the hydrogen-containing silicone oil is 20 mPa·s to 100 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 0.01% to 1%.

6. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The viscosity of the vinyl silicone oil is 100 mPa·s to 500 mPa·s, and the vinyl content of the vinyl silicone oil is 0.1% to 1%.

7. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The thermally conductive powder includes any one or more of aluminum oxide powder, zinc oxide powder, boron nitride powder, aluminum nitride powder, aluminum powder, silver powder, diamond powder, graphite, graphene and carbon nanotubes.

8. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The raw material also includes 0.1wt% to 3wt% of an auxiliary agent, and the auxiliary agent includes any one or more of a high temperature resistant auxiliary agent, a tackifier, an antioxidant and an anti-aging agent.

9. A thermally conductive gasket, characterized in that: The thermally conductive gasket is prepared according to the method for preparing a thermally conductive gasket according to any one of claims 1 to 8.

10. An optical module, characterized in that: The optical module comprises the thermally conductive pad according to claim 9.