Environment-friendly native fiberboard, preparation method and application
Through alkali treatment and graft modification, bamboo fibers can be treated with reduced water absorption and enhanced antibacterial and mildew resistance, which solves the problem of traditional fiber boards expanding and molding in humid environments, and achieves stronger waterproof and mildew resistance and mildew resistance. Longer service life.
Patent Information
- Application Number
- CN202411492264.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional fiber boards are prone to expand and mold in humid environments, affecting their service life.
Bamboo fibers are treated with alkali accelerated rupture and depolymerization, and graft modification is carried out by (3-aminopropyl)trimethoxysilane and 4-carboxynaphthalene-1-boric acid to reduce the water absorption of the fibers and introduce boron-based groups at the same time and naphthalene rings to enhance antibacterial and mildew resistance.
The modified bamboo fiber boards produced have stronger waterproof and mildew resistance and longer service life, and are environmentally friendly and safe.
Smart Images

Figure CN118994933A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiberboards, and in particular to an environmentally friendly virgin fiberboard, a preparation method and application thereof. Background Art
[0002] Fiberboard is a new type of building material with many advantages, including environmental protection, fire prevention, moisture resistance, light weight and high strength, heat insulation and sound insulation. This board is usually made of wood fiber, Portland cement, quartz sand and other auxiliary materials, and is processed through fully automated processes such as precise batching, molding, pressurization and pressurization maintenance. Due to its environmental protection characteristics, fiber cement board does not contain asbestos and is a green and energy-saving building wall material. The construction process of fiberboard includes base treatment, line positioning, installation of base board, installation of support parts, filling materials, installation of decorative layer, closing treatment and cleaning and maintenance. During the construction process, it is necessary to pay attention to the firmness of the fiberboard base to ensure the overall stability and safety of the wall surface, and at the same time protect the wall surface, fiberboard base and decorative layer materials to avoid damage. The application range of fiberboard is very wide, suitable for various industrial and civil buildings, such as office buildings, moisture-proof, fire-proof, partition walls, exterior walls, floor slabs in humid environments. They are also widely used in various art buildings such as offices, hotels, schools, containers, shopping malls, villas, theaters, playgrounds, etc.
[0003] CN106272869A discloses an environmentally friendly antibacterial and mildew-proof composite fiberboard and a preparation method thereof, which is made of the following raw materials in parts by weight: 5-8 parts of poplar leaves, 5-10 parts of wood flour, 5-9 parts of crop straw, 3-6 parts of diatomaceous earth, 7-15 parts of polyurethane, 5-10 parts of polyether, 5-8 parts of acetate fiber, 2-4 parts of DL-benzyl succinic acid, 3-5 parts of ethylene glycol monostearate, 1-3 parts of melamine phosphate, 2-6 parts of styrene acrylic emulsion, 1-4 parts of silane coupling agent, 2-3 parts of antioxidant, and 2-5 parts of adhesive. The prepared environmentally friendly antibacterial and mildew-proof composite fiberboard is stable in nature, mildew-proof, environmentally friendly, and pollution-free.
[0004] CN112356208 A belongs to the technical field of fiberboard manufacturing, and relates to a waterproofing agent, and in particular to a fiberboard waterproofing agent, which includes raw materials by weight: 40-60 parts of wax, 10-20 parts of polyvinyl alcohol, 5-10 parts of silicone, and 25-30 parts of low-density polyethylene. The invention also discloses the preparation of the waterproofing agent and its application in waterproof fiberboard. The invention adopts a new waterproofing agent and a waterproof adhesive, and the prepared fiberboard is low in formaldehyde and environmentally friendly, has good moisture-proof performance, high board bonding strength, and has certain flame retardant functions, low production cost, and high cost performance. It can effectively solve the current problems of poor binding ability of waterproofing agents, high melamine content in adhesives, and high cost, and improve the problems of thickness expansion and deformation of boards under high temperature and high humidity environments.
[0005] In the prior art, fiberboard is generally manufactured by mixing wood cellulose or plant fiber with an adhesive, followed by a pressurization and heating process. Due to the inherent structure and chemical properties of these natural fiber materials, they are naturally highly absorbent and can easily absorb surrounding moisture. Therefore, traditional fiberboards usually exhibit high hygroscopicity and are prone to swelling and mold in a humid environment, which greatly affects the use of fiberboards. Summary of the invention
[0006] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide an environmentally friendly virgin fiber board, a preparation method and application thereof.
[0007] Cellulose fibers, such as cotton, linen, and bamboo, are long-chain polymers composed of glucose units, with abundant hydroxyl (-OH) groups that can form hydrogen bonds with water molecules, thereby attracting and retaining moisture. In addition, the porous and hollow structure of these fibers provides a large amount of surface area and capillary effect, allowing water molecules to be quickly absorbed and diffuse inside the fiber. The amorphous areas and rough surfaces in the fibers also provide more contact and binding opportunities for water molecules. The invention provides a modified bamboo fiber. Firstly, the bamboo fiber is treated with alkali to accelerate the fiber rupture and depolymerization, so that the fiber is decomposed into smaller fibers, and the internal structure thereof is destroyed, thereby affecting the water absorption thereof. Then, (3-aminopropyl)trimethoxysilane and 4-carboxynaphthalene-1-boric acid are used for grafting modification, so that a large number of hydrophilic hydroxyl groups are replaced, resulting in a decrease in hydrophilicity, thereby becoming hydrophobic. The boron groups and naphthalene rings introduced after the grafting can give the material good antibacterial and mildew-proof effects and stronger rigidity. The boron compound has an interfering effect on the cell structure and physiological function of microorganisms, so that bacteria, fungi and other microorganisms can be inhibited or killed. The modified bamboo fiber is applied as the main raw material to the preparation of fiberboard, which is not only more environmentally friendly, but also can improve the waterproof and mildew-proof properties of the board, so that the fiberboard has a longer service life.
[0008] To achieve the above-mentioned object, the present invention provides an environmentally friendly virgin fiber board, comprising the following components in parts by weight: 50-80 parts of modified bamboo fiber, 5-8 parts of urea-formaldehyde resin, 10-20 parts of filler and 0.05-0.2 parts of curing agent.
[0009] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. Crush 80-100 parts of bamboo fiber and immerse them in 4 times the volume of 5wt% sodium hydroxide solution, heat to 100-110°C, treat for 0.5-1h and filter, dry and mix with anhydrous ethanol and ammonia water, disperse evenly and heat to 50-60°C, add 50-80 parts of (3-aminopropyl)trimethoxysilane dropwise, stir for 2-3h and filter, wash the residue with water until neutral and use in the next step; X2. Disperse the product of the previous step in 500-1000 parts of 0.1 mol / L PBS buffer, add 150-200 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 40-80 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 20-30 hours, then add 60-120 parts of 4-carboxynaphthalene-1-boric acid, stir for 12-20 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber.
[0010] Furthermore, the filler is magnesium sulfate whisker or one of silicon dioxide and calcium carbonate.
[0011] Furthermore, the curing agent is a 20-25wt% ammonium chloride solution.
[0012] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps: S1, mixing urea-formaldehyde resin and curing agent to obtain glue solution, then mixing with modified bamboo fiber and filler, and drying to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0013] Furthermore, the drying is performed to a moisture content of less than 10%.
[0014] Furthermore, the temperature of the hot pressing is 165-175°C.
[0015] Furthermore, the hot pressing time is 30-40s / mm.
[0016] Furthermore, the hot pressing pressure is 3-3.5 MPa.
[0017] The present invention also provides an application of an environmentally friendly virgin fiberboard in prefabricated buildings and rapid wall assembly.
[0018] Beneficial effects of the present invention: 1. Compared with the prior art, the fiberboard prepared by the present invention has the advantages of high strength, waterproof and mildew-proof, safety and environmental protection, and also has wide industrial promotion value and longer service life.
[0019] 2. The present invention accelerates the rupture and depolymerization of bamboo fibers by alkali treatment, thereby decomposing them into smaller fibers and destroying their internal structures. Waterproof and mildew-proof modified bamboo fibers are then obtained by grafting and modifying them with (3-aminopropyl)trimethoxysilane and 4-carboxynaphthalene-1-boric acid. Applying the modified bamboo fibers as the main raw material to the preparation of fiberboards is not only more environmentally friendly, but also can improve the waterproof and mildew-proof properties of the boards, thereby extending the service life of the fiberboards. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a photo of a sample prepared by the present invention. DETAILED DESCRIPTION
[0021] The invention provides an environmentally friendly virgin fiber board, comprising the following components: modified bamboo fiber, urea-formaldehyde resin, filler and curing agent. The modified bamboo fiber is the main component of the board, providing the basic structure and strength of the board. The modified bamboo fiber is enhanced in fiber properties such as strength, water resistance and mildew resistance through alkali treatment and grafting modification, making the board stronger and more durable. Urea-formaldehyde resin is used as an adhesive to fix the bamboo fiber into shape and provide a certain bonding strength. Fillers such as magnesium sulfate whiskers, silicon dioxide or calcium carbonate can increase the density and stability of the board, and also help to improve the water resistance and strength of the board. The addition of fillers can also reduce the amount of resin used, thereby reducing costs. The curing agent is used to promote the curing process of urea-formaldehyde resin, so that the board has better stability and mechanical properties after molding. The use of curing agent can speed up the production cycle and improve production efficiency. Through this formula and process, a fiber board that is both environmentally friendly and has good performance can be prepared to meet the needs of furniture manufacturing, construction and interior decoration.
[0022] Urea-formaldehyde resin, product number: 5632, Zhengzhou Hengtong Chemical Company.
[0023] Bamboo fiber, 20 mesh, Longmen County Shenglong Bamboo and Wood Craft Products Factory.
[0024] 4-Carboxynaphthalene-1-boronic acid, 4-borononaphthalene-1-carboxylic acid, CAS: 332398-57-9.
[0025] Silicon dioxide, 100~200nm. Example 1
[0026] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 7 parts of urea-formaldehyde resin and 0.1 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 70 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0027] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral and used in the next step; X2. Disperse the product of the previous step in 1000 parts of 0.1 mol / L PBS buffer, add 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 45 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 24 hours, then add 100 parts of 4-carboxynaphthalene-1-boric acid, stir for 16 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber. Example 2
[0028] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 5 parts of urea-formaldehyde resin and 0.07 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 50 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0029] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral and used in the next step; X2. Disperse the product of the previous step in 1000 parts of 0.1 mol / L PBS buffer, add 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 45 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 24 hours, then add 100 parts of 4-carboxynaphthalene-1-boric acid, stir for 16 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber. Example 3
[0030] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 6 parts of urea-formaldehyde resin and 0.086 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 60 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0031] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral and used in the next step; X2. Disperse the product of the previous step in 1000 parts of 0.1 mol / L PBS buffer, add 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 45 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 24 hours, then add 100 parts of 4-carboxynaphthalene-1-boric acid, stir for 16 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber. Example 4
[0032] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 8 parts of urea-formaldehyde resin and 0.11 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 80 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0033] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral and used in the next step; X2. Disperse the product of the previous step in 1000 parts of 0.1 mol / L PBS buffer, add 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 45 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 24 hours, then add 100 parts of 4-carboxynaphthalene-1-boric acid, stir for 16 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber. Comparative Example 1
[0034] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 7 parts of urea-formaldehyde resin and 0.1 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 70 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0035] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral to obtain modified bamboo fiber. Comparative Example 2
[0036] A method for preparing an environmentally friendly virgin fiberboard comprises the following steps, measured in parts by weight: S1, 7 parts of urea-formaldehyde resin and 0.1 parts of 20wt% ammonium chloride solution are mixed to obtain a glue solution, and then mixed evenly with 70 parts of modified bamboo fiber and 10 parts of silicon dioxide, and dried to a water content of 8% to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed at 170°C, 3MPa, and 30s / mm to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
[0037] The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. 100 parts of bamboo fiber were crushed and immersed in 4 times the volume of 5wt% sodium hydroxide solution, heated to 100°C, treated for 1 hour and filtered, dried and mixed with 400 parts of anhydrous ethanol and 200 parts of 5wt% ammonia water, dispersed evenly and heated to 50°C, 80 parts of (3-aminopropyl)trimethoxysilane were added dropwise, stirred for 2 hours and filtered, and the residue was washed with water until neutral and used in the next step; X2. Disperse the product of the previous step in 1000 parts of 0.1 mol / L PBS buffer, add 180 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 45 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 24 hours, then add 76.4 parts of 4-carboxyphenylboric acid, stir for 16 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber. Test Example 1
[0038] With reference to GB / T 11718-2021 "Medium Density Fiberboard", the static bending strength, internal bonding strength and water absorption thickness expansion rate of the environmentally friendly virgin fiber boards prepared in the embodiments and the control examples were tested, and with reference to GB / T 39600-2021 "Formaldehyde Emission Classification of Artificial Boards and Their Products", the formaldehyde emission level of the environmentally friendly virgin fiber boards prepared in the embodiments and the control examples was tested. The specific results are shown in Table 1.
[0039] Table 1 Performance test results of environmentally friendly virgin fiberboard
[0040] From the test data of Table 1, it can be seen that the environmentally friendly original fiberboard prepared by the present invention has good static bending strength and internal bonding strength, as well as low water absorption thickness expansion rate, and the formaldehyde emission has also reached the E0 level, which is environmentally friendly and very safe. And from the comparison of the embodiment and the reference example 1, it can be found that the fiberboard strength and water absorption thickness expansion rate of the reference example 1 are significantly worse than those of the embodiment, which may be due to the fact that although the alkali-treated bamboo fiber can accelerate the rupture and depolymerization of the fiber, so that it is decomposed into smaller fibers, destroying its internal structure, thereby affecting its water absorption, but this treatment method is effective for the influence of water absorption, and the surface of the bamboo fiber after treatment still has a large amount of hydrophilic group hydroxyl groups, and in the embodiment, the bamboo fiber after alkali treatment is grafted and modified by (3-aminopropyl) trimethoxysilane and 4-carboxynaphthalene-1-boric acid, so that a large amount of hydrophilic hydroxyl groups are replaced, resulting in a decrease in hydrophilicity, thereby becoming hydrophobic, and the boron group and naphthalene ring introduced after grafting can give the material good antibacterial and mildew-proof effects and stronger rigidity, resulting in better strength of the fiberboard, and water absorption is also significantly reduced. Compared with Example 1, Control Example 2 uses 4-carboxyphenylboric acid instead of 4-carboxynaphthalene-1-boric acid. The naphthalene ring is more rigid than the benzene ring, which may be the reason why the strength of the fiberboard in Example 1 is higher than that in Control Example 2. From the test data, it can be seen that the various properties of the fiberboard in Example 1 are the best among all the examples, which shows that the ratio of Example 1 is more reasonable. Test Example 2
[0041] With reference to LY / T2230-2013 "Evaluation of Anti-mildew Performance of Artificial Boards", the fiberboards prepared in the embodiments and the control examples were tested for anti-mildew, and the fiberboards were graded according to the growth of mold. Grade 0 represents no mold growth on the surface, and no mold growth was observed under a low-power biological optical microscope. Grade 1 represents a small amount of hyphae on the surface of the specimen, but the infected area is ≤10%. Grade 2 represents slight growth of mold hyphae, and the infected area on the surface of the specimen is greater than 10% but less than 30%. Grade 3 represents moderate growth of mold hyphae, and the infected area on the surface of the specimen is greater than 30% but less than 60%. Grade 4 represents severe growth of mold hyphae, and the infected area on the surface of the specimen is greater than 60%. The specific results are shown in Table 2.
[0042] Table 2 Test results of anti-mildew performance of environmentally friendly virgin fiberboard
[0043] As can be seen from the test results of Table 2, the environmentally friendly original fiber board prepared by the present invention has a strong mildew resistance grade. This may be due to the fact that the present invention accelerates the rupture and depolymerization of the fiber by alkali treatment of bamboo fiber, thereby decomposing it into smaller fibers, destroying its internal structure, thereby affecting its water absorption, and then grafting modification by (3-aminopropyl) trimethoxysilane and 4-carboxynaphthalene-1-boric acid, so that a large number of hydrophilic hydroxyl groups are replaced, resulting in a decrease in hydrophilicity, thereby becoming hydrophobic, and the boron group and naphthalene ring introduced after grafting can give the material good antibacterial and mildew resistance and stronger rigidity, and the boron compound has an interfering effect on the cell structure and physiological function of microorganisms, so it can inhibit or kill bacteria, fungi and other microorganisms, resulting in the prepared fiberboard not being easy to absorb water, so it is not conducive to the growth of mold, and the introduction of boron compounds can further inhibit or kill mold, so the mildew resistance grade is high. The bamboo fiber in Reference Example 1 is only treated with alkali, which is easier to absorb water than the embodiment, and no boron compound is introduced, so the mildew resistance grade is poor.
[0044] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. An environmentally friendly virgin fiberboard, characterized in that: The invention comprises the following components in parts by weight: 50-80 parts of modified bamboo fiber, 5-8 parts of urea-formaldehyde resin, 10-20 parts of filler and 0.05-0.2 parts of curing agent.
2. The environmentally friendly virgin fiber board according to claim 1, characterized in that: The preparation method of the modified bamboo fiber comprises the following steps, measured in parts by weight: X1. Crush 80-100 parts of bamboo fiber and immerse them in 4 times the volume of 5wt% sodium hydroxide solution, heat to 100-110°C, treat for 0.5-1h and filter, dry and mix with anhydrous ethanol and ammonia water, disperse evenly and heat to 50-60°C, add 50-80 parts of (3-aminopropyl)trimethoxysilane dropwise, stir for 2-3h and filter, wash the residue with water until neutral and use in the next step; X2. Disperse the product of the previous step in 500-1000 parts of 0.1 mol / L PBS buffer, add 150-200 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, stir evenly, then add 40-80 parts of N-hydroxysuccinimide, stir under nitrogen atmosphere and room temperature for 20-30 hours, then add 60-120 parts of 4-carboxynaphthalene-1-boric acid, stir for 12-20 hours and filter, wash the residue with water until neutral and then dry to obtain modified bamboo fiber.
3. The environmentally friendly virgin fiber board according to claim 1, characterized in that: The filler is one of magnesium sulfate whisker, silicon dioxide and calcium carbonate.
4. The environmentally friendly virgin fiber board according to claim 1, characterized in that: The curing agent is a 20-25wt% ammonium chloride solution.
5. The method for preparing the environmentally friendly virgin fiber board according to any one of claims 1 to 4, characterized in that: The steps include: S1, mixing urea-formaldehyde resin and curing agent to obtain glue solution, then mixing with modified bamboo fiber and filler, and drying to obtain a mixed material; S2. The mixed material is spread in a forming mold and hot-pressed to obtain a plate. After the plate is cooled to room temperature, it is trimmed and sanded before inspection and storage.
6. The method for preparing the environmentally friendly virgin fiber board according to claim 5, characterized in that: The drying is drying to a moisture content of less than 10%.
7. The method for preparing the environmentally friendly virgin fiber board according to claim 5, characterized in that: The temperature of the hot pressing is 165-175°C.
8. The method for preparing the environmentally friendly virgin fiber board according to claim 5, characterized in that: The hot pressing time is 30-40s / mm.
9. The method for preparing the environmentally friendly virgin fiber board according to claim 5, characterized in that: The hot pressing pressure is 3-3.5 MPa.
10. Application of the environmentally friendly virgin fiber board according to any one of claims 1 to 4 in prefabricated buildings and rapid wall assembly.
Citation Information
Patent Citations
Full-degradation natural fibre / polylactic acid composite material and preparation method thereof
CN101121813A
Method for preparing polyethylene-based thermoplastic wood-plastic composite material
CN101230165A
Long-acting mould-proof wood plastic composite material and preparation method thereof
CN101767362A
Bamboo medium density fiberboard
CN105522636A