Preparation method of high-strength wear-resistant ceramic coating

High-strength wear-resistant ceramic coatings are prepared by mixing and baking materials such as high-strength wear-resistant ceramic tiles, which solves the problems of complex construction operations, unstable quality and high cost, and improves the service life and high temperature resistance of the material.

CN118994948AInactive Publication Date: 2024-11-22HENAN HONGYAN REFRACTORY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088144.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing wear-resistant ceramic coatings are troublesome during construction, with unstable quality, high cost, and poor strength during use, which affects the life of high-temperature equipment.

Method used

High-strength wear-resistant ceramic coatings are prepared by using high-aluminum ceramic brick-lined particles, cyanite particles, oxide powders, composite binders and composite coagulation agents as raw materials. The high-strength wear-resistant ceramic coatings are added to the solid bonding agent and High-efficiency coagulant to improve material strength and high temperature resistance.

Benefits of technology

It effectively solves the problems of complex construction operations, unstable quality and high cost, improves the service life of the materials and high temperature resistance, and reduces transportation and construction costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength wear-resistant ceramic coating, and relates to the field of refractory plastic materials, the preparation method of the high-strength wear-resistant ceramic coating comprises the following steps: S1, preparing raw materials of the ceramic coating; the preparation method comprises the following steps: firstly, preparing high-aluminum ceramic lining brick particles, kyanite particles, oxide micro powder, a composite binder and a composite coagulant, and then separately preparing the high-aluminum ceramic lining brick particles, the kyanite particles, the oxide micro powder, the composite binder and the composite coagulant into four groups for later use; according to the invention, the high-aluminum ceramic aggregate, the alumina micro-powder binder and the like are mixed and then smeared, so that the baked wear-resistant coating has outstanding wear resistance and better overall high temperature resistance, the service life of the product is effectively prolonged, the problem that the existing wear-resistant coating is troublesome to transport is solved, and the overall cost of the material is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of refractory plastics, in particular to a method for preparing a high-strength wear-resistant ceramic coating material. Background Art

[0002] Existing wear-resistant ceramic coatings are mainly made of liquid sodium silicate, combined with refractory ceramic aggregate and refractory fine material, which are divided into wear-resistant ceramic dry materials and binders, which are transported to the construction site together and stirred and applied on site when used.

[0003] The existing wear-resistant ceramic coating has the following disadvantages in terms of construction process and use effect: First, the on-site construction operation is relatively troublesome, and the binder and other additives cannot be directly mixed, which increases the burden on the on-site staff and easily causes unstable quality. Second, as an important component of the wear-resistant ceramic coating, the liquid sodium silicate accounts for about 20% of the total weight, which is included in the weight of the entire wear-resistant ceramic material, which increases the cost. Third, the existing wear-resistant ceramic coating uses relatively low-grade electric porcelain bottles as aggregates, which are mostly in flaky form after being crushed. The bulk density of the entire material is low, the strength is poor during use, and the powder material selection is relatively low-end, which seriously reduces the service life of high-temperature equipment.

[0004] Therefore, those skilled in the art provide a method for preparing a high-strength wear-resistant ceramic coating material to solve the problems raised in the above background technology. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a high-strength wear-resistant ceramic coating material, so as to solve the problems that the existing wear-resistant ceramic coating material proposed in the above background technology has the following disadvantages in the construction process and use effect: first, the on-site construction operation is relatively troublesome, and the additives such as the binder cannot be directly mixed well, which increases the burden on the on-site staff and easily causes unstable quality. Second, as an important component of the wear-resistant ceramic coating, the liquid sodium silicate accounts for about 20% of the total weight, which is included in the weight of the entire wear-resistant ceramic material, which increases the cost. Third, the existing wear-resistant ceramic coating material uses relatively low-grade electric porcelain bottles as aggregates, which are mostly in flaky form after being crushed. The bulk density of the entire material is low, the strength is poor during use, and the powder material selection is relatively low-end, which seriously reduces the service life of high-temperature equipment.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a high-strength wear-resistant ceramic coating material, the method comprising the following steps:

[0008] S1: raw material preparation step of the ceramic coating material, first prepare high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant, then prepare four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant separately for standby use;

[0009] S2: Raw material preparation step of ceramic coating material, firstly, four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant are mixed in proportion to each group, and then the obtained raw materials are mixed and stirred evenly in four groups, and then water is added to the four groups of finished materials for stirring, and then the construction is applied. The finished materials can be added with drinking water at a ratio of 10% of the weight of each group of mixed raw materials, and then each group of coating materials is baked, and finally the coating materials are cooled to obtain a shaped coating material;

[0010] S3: The steps of selecting the components and weight percentages of the wear-resistant ceramic coating material, wherein 20%-30% of the ceramic particles with a diameter of 5-3mm are selected, 15%-20% of the ceramic particles with a diameter of 1-3mm are selected, 10%-20% of the ceramic particles with a diameter of 0-1mm are selected, 15%-25% of ceramic fine powder are selected, 5%-10% of kyanite is selected, 6%-15% of alumina micropowder is selected, 5%-10% of solid binder is selected, 2%-5% of coagulant is selected and 0.2% of water reducer is selected.

[0011] S4: The step of selecting physical and chemical indicators, the ceramic particles are mixed in proportion with particle sizes of 5-3mm, 3-1mm and 1-0mm, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2, R2O(%)≤0.5, bulk density (g / cm3)≥2.4 and water absorption rate (%)≤2.5; the ceramic fine powder is mixed in proportion with a fineness of -200 mesh, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2 and R2O(%)≤0.5; the kyanite is 60 mesh fine sand, Al2O3(%)≥52, SiO2(%)≤36, Fe2O3(%)≤0.9 and R2O(%)≤0.8; the alumina micropowder It is mixed in proportion with a particle size of -800 mesh, and its physical and chemical indicators are Al2O3(%) ≥99.2, Fe2O3(%) ≤0.1 and R2O(%) ≤0.5; the solid binder is mixed with fast-dissolving sodium silicate, and its physical and chemical indicators are modulus 2.85, SiO2(%) ≥55, Na2O3(%) ≤20, dissolution rate ≤180s, specific gravity 0.4-0.7g / cm3, and 100 mesh screening rate ≥98%; the coagulant is mixed with sodium fluorosilicate, and its physical and chemical indicators are dissolution rate ≤100s, specific gravity 2.65g / cm3, and 180 mesh screening rate ≥98%; the water reducer is sodium tripolyphosphate with a dissolution rate ≤100s, a specific gravity of 2.60g / cm3, and a fineness of 0-2mm.

[0012] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the first group of the four groups prepares 400-650 parts of high-alumina ceramic lining brick particles, 150-250 parts of kyanite particles, 150-200 parts of oxide powder, 100-200 parts of composite binder and 50-100 parts of composite accelerator.

[0013] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the second group of the four groups prepares 500 parts of high-alumina ceramic lining brick particles, 150 parts of kyanite particles, 150 parts of oxide powder, 150 parts of composite binder and 50 parts of composite accelerator.

[0014] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the third group of the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 150 parts of oxide powder, 100 parts of composite binder and 50 parts of composite coagulant.

[0015] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the fourth group among the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 100 parts of oxide powder, 150 parts of composite binder and 50 parts of composite accelerator.

[0016] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the diameter size of the high-alumina ceramic lining brick particles can be selected between 3mm-5mm, 3mm-2mm, 2mm-1mm, or 1mm-0mm.

[0017] As a preferred embodiment of the present invention: in the raw material preparation step of the ceramic coating material, the diameter of the kyanite particles is 60 mesh, and the oxide powder is a mixture of several types of alumina powder.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The invention discloses a method for preparing a high-strength wear-resistant ceramic coating material, which can prepare a high-strength wear-resistant ceramic coating material, belongs to the high-temperature refractory material industry, and is applied to the flue of a fluidized bed boiler in a power plant, a hot air duct, a tortoise shell mesh and other linings for coating operations. The high-temperature equipment can be effectively protected to operate normally at a high temperature below 1100 degrees, and can withstand the scouring caused by the high-speed hot air flow, which solves the problems of the current coating material being cumbersome to use in construction, unstable quality, and unreasonable cost allocation, and improves the service life of the material as a whole. By adding a solid binder and a high-efficiency coagulant, the overall cost of the material is reduced, the transportation trouble problem and the complex construction operation problem are solved, and the binder is condensed and combined by adding oxide micropowder, so that the material strength is greatly improved. The high-strength wear-resistant ceramic coating material and the preparation method thereof are applied after mixing high-aluminum ceramic aggregate and alumina micropowder binder, and the wear-resistant coating after baking has outstanding wear resistance and good overall high temperature resistance, which effectively prolongs the service life of the product, solves the current wear-resistant coating material transportation trouble problem, and reduces the overall cost of the material. DETAILED DESCRIPTION

[0020] In an embodiment of the present invention, a method for preparing a high-strength wear-resistant ceramic coating material is provided, and the method for preparing a high-strength wear-resistant ceramic coating material comprises the following steps:

[0021] S1: raw material preparation step of the ceramic coating material, first prepare high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant, then prepare four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant separately for standby use;

[0022] S2: Raw material preparation step of ceramic coating material, firstly, four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant are mixed in proportion to each group, and then the obtained raw materials are mixed and stirred evenly in four groups, and then water is added to the four groups of finished materials for stirring, and then the construction is applied. The finished materials can be added with drinking water at a ratio of 10% of the weight of each group of mixed raw materials, and then each group of coating materials is baked, and finally the coating materials are cooled to obtain a shaped coating material;

[0023] S3: The steps of selecting the components and weight percentages of the wear-resistant ceramic coating material, wherein 20%-30% of the ceramic particles with a diameter of 5-3mm are selected, 15%-20% of the ceramic particles with a diameter of 1-3mm are selected, 10%-20% of the ceramic particles with a diameter of 0-1mm are selected, 15%-25% of ceramic fine powder are selected, 5%-10% of kyanite is selected, 6%-15% of alumina micropowder is selected, 5%-10% of solid binder is selected, 2%-5% of coagulant is selected and 0.2% of water reducer is selected.

[0024] S4: The step of selecting physical and chemical indicators, the ceramic particles are mixed in proportion with particle sizes of 5-3mm, 3-1mm and 1-0mm, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2, R2O(%)≤0.5, bulk density (g / cm3)≥2.4 and water absorption rate (%)≤2.5; the ceramic fine powder is mixed in proportion with a fineness of -200 mesh, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2 and R2O(%)≤0.5; the kyanite is 60 mesh fine sand, Al2O3(%)≥52, SiO2(%)≤36, Fe2O3(%)≤0.9 and R2O(%)≤0.8; the alumina micropowder It is mixed in proportion with a particle size of -800 mesh, and its physical and chemical indicators are Al2O3(%) ≥99.2, Fe2O3(%) ≤0.1 and R2O(%) ≤0.5; the solid binder is mixed with fast-dissolving sodium silicate, and its physical and chemical indicators are modulus 2.85, SiO2(%) ≥55, Na2O3(%) ≤20, dissolution rate ≤180s, specific gravity 0.4-0.7g / cm3, and 100 mesh screening rate ≥98%; the coagulant is mixed with sodium fluorosilicate, and its physical and chemical indicators are dissolution rate ≤100s, specific gravity 2.65g / cm3, and 180 mesh screening rate ≥98%; the water reducer is sodium tripolyphosphate with a dissolution rate ≤100s, a specific gravity of 2.60g / cm3, and a fineness of 0-2mm.

[0025] It can produce high-strength wear-resistant ceramic coatings, which belong to the high-temperature refractory industry and are used in the lining of fluidized bed boiler flues, hot air ducts, tortoise shell mesh, etc. in power plants for coating operations. It can effectively protect high-temperature equipment from operating normally at temperatures below 1100 degrees, and can withstand the erosion caused by high-speed hot air flow, solving the current problems of tedious use of coatings in construction, unstable quality, and unreasonable cost allocation, and overall improving the service life of the materials.

[0026] Example 1

[0027] In this embodiment, the components and weight percentages of the wear-resistant ceramic coating are: ceramic particles 5mm-mm 15% 3mm-1mm 20% 0mm-1mm 25% oxide powder 10% ceramic fine powder 20% kyanite 8% solid binder 8% accelerator 3% water reducer 0.2%.

[0028] The mixture prepared in the above proportions was stirred for 5 minutes, 15% of the weight of water was added and then stirred for 8 minutes, and vibrated and cast into a sample block of 40mm×40mm×160mm, cured for 24 hours, baked at 110°C for 24 hours, and fired at a high temperature of 1100°C for 3 hours.

[0029] The product performance test results are:

[0030] After baking at 110℃×24h, the volume density is 2.45g / cm 3 ;

[0031] After baking at 110℃×24h, the cold flexural strength is 11Mpa;

[0032] Cold compressive strength after baking at 110℃×24h: 65Mpa;

[0033] After baking at 1100℃×24h, the cold flexural strength is 17Mpa;

[0034] After baking at 1100℃×24h, the cold compressive strength is 96Mpa.

[0035] Example 2

[0036] In this embodiment, the components and weight percentages of the wear-resistant ceramic coating are: ceramic particles 5mm-mm 20% 3mm-1mm 15% 0mm-1mm 20% oxide powder 10% ceramic fine powder 25% kyanite 8% solid binder 8% accelerator 3% water reducer 0.2%.

[0037] The mixture prepared in the above proportions was stirred for 5 minutes, 15% of the weight of water was added and then stirred for 8 minutes, and vibrated and cast into a sample block of 40mm×40mm×160mm, cured for 24 hours, baked at 110°C for 24 hours, and fired at a high temperature of 1100°C for 3 hours.

[0038] The product performance test results are:

[0039] After baking at 110℃×24h, the volume density is 2.5g / cm 3 ;

[0040] After baking at 110℃×24h, the cold flexural strength is 9Mpa;

[0041] Cold compressive strength after baking at 110℃×24h: 55Mpa;

[0042] After baking at 1100℃×24h, the cold flexural strength is 15Mpa;

[0043] After baking at 1100℃×24h, the cold compressive strength is 86Mpa.

[0044] Example 3

[0045] In this embodiment, the components and weight percentages of the wear-resistant ceramic coating are: ceramic particles 5mm-mm 18% 3mm-1mm 17% 0mm-1mm 22% oxide powder 7% ceramic fine powder 26% kyanite 8% solid binder 8% accelerator 3% water reducer 0.2%.

[0046] The mixture prepared in the above proportions was stirred for 5 minutes, 15% of the weight of water was added and then stirred for 8 minutes, and vibrated and cast into a sample block of 40mm×40mm×160mm, cured for 24 hours, baked at 110°C for 24 hours, and fired at a high temperature of 1100°C for 3 hours.

[0047] The product performance test results are:

[0048] After baking at 110℃×24h, the volume density is 2.55g / cm 3 ;

[0049] After baking at 110℃×24h, the cold flexural strength is 8Mpa;

[0050] Cold compressive strength after baking at 110℃×24h: 55Mpa;

[0051] After baking at 1100℃×24h, the cold flexural strength is 13Mpa;

[0052] After baking at 1100℃×24h, the cold compressive strength is 75Mpa.

[0053] In the raw material preparation step of the ceramic coating material, the first group of the four groups prepares 400-650 parts of high-alumina ceramic lining brick particles, 150-250 parts of kyanite particles, 150-200 parts of oxide powder, 100-200 parts of composite binder and 50-100 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the second group of the four groups prepares 500 parts of high-alumina ceramic lining brick particles, 150 parts of kyanite particles, 150 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the third group of the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 150 parts of oxide powder, 100 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the fourth group of the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 100 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the diameter size of the high-alumina ceramic lining brick particles can be selected from a diameter size between 3mm-5mm, a diameter size between 3mm-2mm, a diameter size between 2mm-1mm, or a diameter size between 1mm-0mm. In the raw material preparation step of the ceramic coating material, the diameter size of the kyanite particles is 60 mesh, and the oxide powder is a mixture of several types of alumina powder.

[0054] By adding solid binders and high-efficiency coagulants, the overall cost of materials is reduced, the problem of troublesome transportation and complicated construction operations is solved, and the binder is condensed and bonded by adding oxide micropowder, so that the strength of the material is greatly improved. The high-strength wear-resistant ceramic coating and its preparation method are applied after mixing high-alumina ceramic aggregate and alumina micropowder binder. The wear-resistant coating after baking has outstanding wear resistance and good overall high temperature resistance, which effectively extends the service life of the product, solves the problem of the current wear-resistant coating transportation troubles, and reduces the overall cost of materials.

[0055] The working principle of the present invention is: the preparation method of the high-strength wear-resistant ceramic coating material comprises the following steps:

[0056] S1: The raw material preparation step of the ceramic coating material, first prepare high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant, and then prepare four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant separately for standby use; In the raw material preparation step of the ceramic coating material, the first group of the four groups prepares 400-650 parts of high-alumina ceramic lining brick particles, 150-250 parts of kyanite particles, 150-200 parts of oxide powder, 100-200 parts of composite binder and 50-100 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the second group of the four groups prepares 500 parts of high-alumina ceramic lining brick particles, 150 parts of kyanite particles, 150 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the third group of the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 150 parts of oxide powder, 100 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the fourth group of the four groups prepares 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 100 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant. In the raw material preparation step of the ceramic coating material, the diameter size of the high-alumina ceramic lining brick particles can be selected from a diameter size between 3mm-5mm, a diameter size between 3mm-2mm, a diameter size between 2mm-1mm, or a diameter size between 1mm-0mm. In the raw material preparation step of the ceramic coating material, the diameter size of the kyanite particles is 60 mesh, and the oxide powder is a mixture of several types of alumina powder.

[0057] S2: Raw material preparation step of ceramic coating material, firstly, four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant are mixed in proportion to each group, and then the obtained raw materials are mixed and stirred evenly in four groups, and then water is added to the four groups of finished materials for stirring, and then the construction is applied. The finished materials can be added with drinking water at a ratio of 10% of the weight of each group of mixed raw materials, and then each group of coating materials is baked, and finally the coating materials are cooled to obtain a shaped coating material;

[0058] S3: The steps of selecting the components and weight percentages of the wear-resistant ceramic coating material, wherein 20%-30% of the ceramic particles with a diameter of 5-3mm are selected, 15%-20% of the ceramic particles with a diameter of 1-3mm are selected, 10%-20% of the ceramic particles with a diameter of 0-1mm are selected, 15%-25% of ceramic fine powder are selected, 5%-10% of kyanite is selected, 6%-15% of alumina micropowder is selected, 5%-10% of solid binder is selected, 2%-5% of coagulant is selected and 0.2% of water reducer is selected.

[0059] S4: The step of selecting physical and chemical indicators, the ceramic particles are mixed in proportion with particle sizes of 5-3mm, 3-1mm and 1-0mm, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2, R2O(%)≤0.5, bulk density (g / cm3)≥2.4 and water absorption rate (%)≤2.5; the ceramic fine powder is mixed in proportion with a fineness of -200 mesh, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2 and R2O(%)≤0.5; the kyanite is 60 mesh fine sand, Al2O3(%)≥52, SiO2(%)≤36, Fe2O3(%)≤0.9 and R2O(%)≤0.8; the alumina micropowder It is mixed in proportion with a particle size of -800 mesh, and its physical and chemical indicators are Al2O3(%) ≥99.2, Fe2O3(%) ≤0.1 and R2O(%) ≤0.5; the solid binder is mixed with fast-dissolving sodium silicate, and its physical and chemical indicators are modulus 2.85, SiO2(%) ≥55, Na2O3(%) ≤20, dissolution rate ≤180s, specific gravity 0.4-0.7g / cm3, and 100 mesh screening rate ≥98%; the coagulant is mixed with sodium fluorosilicate, and its physical and chemical indicators are dissolution rate ≤100s, specific gravity 2.65g / cm3, and 180 mesh screening rate ≥98%; the water reducer is sodium tripolyphosphate with a dissolution rate ≤100s, a specific gravity of 2.60g / cm3, and a fineness of 0-2mm.

[0060] It can prepare high-strength wear-resistant ceramic coatings, which belong to the high-temperature refractory industry and are used for coating operations in the flue of fluidized bed boilers in power plants, hot air ducts, tortoise shell mesh and other linings. It can effectively protect high-temperature equipment from normal operation at high temperatures below 1100 degrees, and can withstand the scouring caused by high-speed hot air flow, solving the problems of tedious use of coatings in construction, unstable quality, and unreasonable cost allocation, and overall improving the service life of the materials. By adding solid binders and high-efficiency coagulants, the overall cost of materials is reduced, the transportation troubles and the complex construction operations are solved, and the material strength is greatly improved by adding oxide micropowders to condense and bind the binders. The high-strength wear-resistant ceramic coating and its preparation method are applied after mixing high-aluminum ceramic aggregates and alumina micropowder binders. The wear-resistant coating after baking has outstanding wear resistance and good overall high temperature resistance, effectively extending the service life of the product, solving the current transportation troubles of wear-resistant coatings, and reducing the overall cost of materials.

[0061] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a high-strength wear-resistant ceramic coating, characterized in that: The preparation method of the high-strength wear-resistant ceramic coating material comprises the following steps: S1: raw material preparation step of the ceramic coating material, first prepare high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant, then prepare four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant separately for standby use; S2: Raw material preparation step of ceramic coating material, firstly, four groups of high-alumina ceramic lining brick particles, kyanite particles, oxide powder, composite binder and composite coagulant are mixed in proportion to each group, and then the obtained raw materials are mixed and stirred evenly in four groups, and then water is added to the four groups of finished materials for stirring, and then the construction is applied. The finished materials can be added with drinking water at a ratio of 10% of the weight of each group of mixed raw materials, and then each group of coating materials is baked, and finally the coating materials are cooled to obtain a shaped coating material; S3: The steps of selecting the components and weight percentages of the wear-resistant ceramic coating material, wherein 20%-30% of the ceramic particles with a diameter of 5-3mm are selected, 15%-20% of the ceramic particles with a diameter of 1-3mm are selected, 10%-20% of the ceramic particles with a diameter of 0-1mm are selected, 15%-25% of ceramic fine powder are selected, 5%-10% of kyanite is selected, 6%-15% of alumina micropowder is selected, 5%-10% of solid binder is selected, 2%-5% of coagulant is selected and 0.2% of water reducer is selected. S4: The step of selecting physical and chemical indicators, the ceramic particles are mixed in proportion with particle sizes of 5-3mm, 3-1mm and 1-0mm, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2, R2O(%)≤0.5, bulk density (g / cm3)≥2.4 and water absorption rate (%)≤2.5; the ceramic fine powder is mixed in proportion with a fineness of -200 mesh, and the physical and chemical indicators are Al2O3(%)≥45, Fe2O3(%)≤1.2 and R2O(%)≤0.5; the kyanite is 60 mesh fine sand, Al2O3(%)≥52, SiO2(%)≤36, Fe2O3(%)≤0.9 and R2O(%)≤0.8; the alumina micropowder It is mixed in proportion with a particle size of -800 mesh, and its physical and chemical indicators are Al2O3(%) ≥99.2, Fe2O3(%) ≤0.1 and R2O(%) ≤0.5; the solid binder is mixed with fast-dissolving sodium silicate, and its physical and chemical indicators are modulus 2.85, SiO2(%) ≥55, Na2O3(%) ≤20, dissolution rate ≤180s, specific gravity 0.4-0.7g / cm3, and 100 mesh screening rate ≥98%; the coagulant is mixed with sodium fluorosilicate, and its physical and chemical indicators are dissolution rate ≤100s, specific gravity 2.65g / cm3, and 180 mesh screening rate ≥98%; the water reducer is sodium tripolyphosphate with a dissolution rate ≤100s, a specific gravity of 2.60g / cm3, and a fineness of 0-2mm.

2. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the first group of the four groups prepares 400-650 parts of high-alumina ceramic lining brick particles, 150-250 parts of kyanite particles, 150-200 parts of oxide powder, 100-200 parts of composite binder and 50-100 parts of composite accelerator.

3. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the second group of the four groups prepared 500 parts of high-alumina ceramic lining brick particles, 150 parts of kyanite particles, 150 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant.

4. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the third group of the four groups prepared 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 150 parts of oxide powder, 100 parts of composite binder and 50 parts of composite coagulant.

5. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the fourth group of the four groups prepared 600 parts of high-alumina ceramic lining brick particles, 100 parts of kyanite particles, 100 parts of oxide powder, 150 parts of composite binder and 50 parts of composite coagulant.

6. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the diameter size of the high-alumina ceramic lining brick particles can be selected from a diameter size between 3mm-5mm, a diameter size between 3mm-2mm, a diameter size between 2mm-1mm, or a diameter size between 1mm-0mm.

7. The method for preparing a high-strength wear-resistant ceramic coating material according to claim 1, characterized in that: In the raw material preparation step of the ceramic coating material, the diameter of the kyanite particles is 60 mesh, and the oxide micropowder is a mixture of several types of alumina micropowder.