DTMS (at) PDA (at) SiO2 (at) CNTs composite material, preparation and application thereof, super-hydrophobic self-repairing anticorrosive paint, coating and preparation thereof
Through the DTMS@PDA@SiO2@CNTs composite material embedded in epoxy resin, the superhydrophobic performance is restored by near-infrared light irradiation, and the problem of superhydrophobic coating being sensitive to harsh environments and limited self-healing in the prior art is solved, and the problem of superhydrophobic coating being sensitive to harsh environments and being limited in self-healing is realized. Metal surfaces have high efficiency and long-lasting superhydrophobic anti-corrosion effects.
Patent Information
- Application Number
- CN202411105229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing superhydrophobic coatings are sensitive to harsh environments and are prone to damage, resulting in loss of superhydrophobicity. Most self-healing methods require heating or are limited by the shape of the substrate and cannot be effectively applied on metal surfaces.
Using DTMS@PDA@SiO2@CNTs composite material, the carboxylated multi-walled carbon nanotubes, tetraethyl silicate and dopamine were grown in situ under alkaline conditions to form nanoSiO2, followed by dodecyl tris Methyloxysilane undergoes oxidation autopolymerization-hydrolysis reaction to form a DTMS@PDA@SiO2@CNTs composite material, embedded in an epoxy resin, and uses near-infrared light irradiation to restore superhydrophobic properties.
It realizes rapid recovery of superhydrophobic properties without heating, is not limited by the matrix shape, and has better mechanical stability and durability, can effectively isolate corrosive media from contact with metal, significantly extending the service life of the coating .
Smart Images

Figure CN118994957A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of super-hydrophobic coatings and self-repairing materials, and in particular to a DTMS@PDA@SiO2@CNTs composite material and its preparation and application, a super-hydrophobic self-repairing anti-corrosion coating, a coating and its preparation. Background Art
[0002] In recent years, super-hydrophobic coatings have shown great industrial potential in the fields of self-cleaning, oil-water separation, corrosion prevention, anti-icing and anti-fogging, drag reduction, etc., especially in corrosion prevention. Metal corrosion worldwide has caused serious waste of resources, economic losses and safety hazards. The preparation of super-hydrophobic coatings on the surface of metal substrates can effectively isolate the metal from the contact with the corrosive medium, thereby greatly reducing the corrosion rate.
[0003] However, most super-hydrophobic coatings are very sensitive to damage, and the effects of harsh environments (such as acid and alkali solutions, organic solvents, wear, washing, ultraviolet radiation, high temperature) may destroy the surface roughness (nanoparticle shedding, substrate wear) or cause an increase in surface energy (decomposition of hydrophobic long chains), and these changes will lead to the loss of super-hydrophobicity, thereby significantly shortening the service life of the super-hydrophobic coating. CN201510475715.7 discloses a method for preparing a self-repairing super-hydrophobic gel, in which a heating method must be used to restore its super-hydrophobic properties, which is limited by the shape of the substrate, and there is no clear explanation whether the gel can be applied to metal surfaces. Summary of the invention
[0004] The object of the present invention is to provide a DTMS@PDA@SiO2@CNTs composite material and its preparation and application, a super-hydrophobic self-repairing anti-corrosion coating, a coating and its preparation. The super-hydrophobic self-repairing anti-corrosion coating provided by the present invention does not need to be heated, and its super-hydrophobic performance is rapidly restored after near-infrared light irradiation, and is not limited by the shape of the substrate. In addition, the super-hydrophobic self-repairing anti-corrosion coating of the present invention also has better mechanical stability and durability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a DTMS@PDA@SiO2@CNTs composite material, comprising the following steps:
[0007] dispersing graphitized carboxylated multi-walled carbon nanotubes in water-a first polar organic solvent to obtain a CNTs dispersion;
[0008] Under alkaline conditions, the CNTs dispersion is mixed with tetraethyl silicate to perform an in-situ growth reaction, and nano-SiO2 is in-situ formed on the surface of the graphitized carboxylated multi-walled carbon nanotubes to obtain SiO2@CNTs;
[0009] Providing a weak alkaline solvent; the pH value of the weak alkaline solvent is 7.5 to 9.5, and the weak alkaline solvent includes water and a second polar organic solvent;
[0010] The SiO2@CNTs, the weak alkaline solvent, dopamine and dodecyltrimethylsilane DTMS are mixed to undergo an oxidative self-polymerization-hydrolysis reaction, wherein the dopamine self-polymerizes on the surface of the SiO2@CNTs to form polydopamine PDA, and simultaneously the DTMS is hydrolyzed to generate silanols that are grafted onto the surface of the SiO2@CNTs to obtain a DTMS@PDA@SiO2@CNTs composite material.
[0011] The present invention provides a DTMS@PDA@SiO2@CNTs composite material prepared by the above-mentioned preparation method, comprising SiO2@CNTs, PDA located on the surface of the SiO2@CNTs, and silanol chains grafted on the SiO2@CNTs; the silanol chains are obtained by hydrolyzing DTMS; the SiO2@CNTs comprise graphitized carboxylated multi-walled carbon nanotubes and nano-SiO2 in-situ grown on the surface of the graphitized carboxylated multi-walled carbon nanotubes.
[0012] The present invention provides the application of the DTMS@PDA@SiO2@CNTs composite material described in the above scheme in a super-hydrophobic coating.
[0013] The present invention provides a super-hydrophobic self-repairing anti-corrosion coating, comprising epoxy resin, the above-mentioned DTMS@PDA@SiO2@CNTs composite material, a curing agent and an organic solvent.
[0014] The invention provides a super-hydrophobic self-repairing anti-corrosion coating, comprising an epoxy resin and a DTMS@PDA@SiO2@CNTs composite material embedded in the epoxy resin.
[0015] The present invention provides a method for preparing the super-hydrophobic self-repairing anti-corrosion coating of the above scheme, comprising the following steps: applying the super-hydrophobic self-repairing anti-corrosion coating of the above scheme to the surface of a metal substrate, and curing the super-hydrophobic self-repairing anti-corrosion coating to obtain the super-hydrophobic self-repairing anti-corrosion coating.
[0016] The present invention provides a super hydrophobic self-repairing anti-corrosion coating, comprising an epoxy resin and a DTMS@PDA@SiO2@CNTs composite material embedded in the epoxy resin. The DTMS@PDA@SiO2@CNTs nanoparticles wrapped in epoxy resin present a uniform and compact agglomeration morphology on the surface of the coating, giving the coating a strong sense of particle roughness, while dopamine self-aggregates to form PDA adsorbed on SiO2 nanoparticles and CNTs nanoparticles, forming a micro-nano dual-scale structure (such as Figure 2As shown in the figure, a large number of micropores are formed between the micro-nano dual-scale structures, which can trap air to form an air cushion to prevent water from penetrating, making the coating have good hydrophobicity. In addition, the hydrolysis chain of DTMS has low surface energy, which is grafted to the surface of SiO2@CNTs, giving the coating a low surface energy, which is beneficial to improving the hydrophobic effect.
[0017] With the help of the classic photothermal agent PDA, the present invention uses SiO2 nanoparticles and carbon nanomaterials to construct a super-hydrophobic surface with strong light absorption in the near-infrared light region. Thanks to the excellent photothermal conversion performance of the coating, the super-hydrophobic property of the composite coating recovers rapidly after near-infrared light irradiation and is not restricted by the shape of the substrate.
[0018] The super-hydrophobic self-healing anti-corrosion coating prepared by the present invention using the DTMS@PDA@SiO2@CNTs composite material as a photothermal filler has super-hydrophobic properties and can effectively isolate the corrosive medium from contact with the metal substrate. The main component of the coating is epoxy resin, which is itself a corrosion-resistant coating. The DTMS embedded in the coating also has good chemical inertness, so that the coating has excellent corrosion resistance.
[0019] In addition, with the assistance of the classic photothermal agent PDA, DTMS@PDA@SiO2@CNTs nanoparticles have strong light absorption in the near-infrared light region. The rough surface morphology of the surface after the coating is cured is its permanent shape. At this time, the polymer molecular chains in the coating are entangled with each other during polymerization, corresponding to the high entropy state, that is, in a thermodynamically stable state, and the superhydrophobic self-healing anti-corrosion coating is in a frozen state. After the coating is damaged, the coating is still in a glassy state, and the activity of the polymer molecular chains is very low, which is manifested as the coating surface cannot be restored to the original micro-nano structure, and the coating loses its superhydrophobic properties. After the coating is exposed to near-infrared irradiation, the coating temperature rises above the glass transition temperature, the molecular chain segments are activated, and the coating changes from a glassy state to a rubbery state. At this time, the activity of the molecular chain is increased again to an extremely high state. According to the principle of entropy increase, the molecular chain conformation will be transformed into a conformation corresponding to the high entropy solid state, that is, the roughness and structure of the coating surface are also restored to the initial state, and the superhydrophobic property of the coating is also repaired.
[0020] In addition, the highly cross-linked epoxy resin in the coating can firmly bind the carbon nanomaterials together. When the peak structure on the surface of the coating is polished smooth, SiO2 and CNTs can still be tightly combined, which is attributed to the bonding effect of PDA. Secondly, CNTs not only have a high Young's modulus and tensile strength, but also because of their one-dimensional tubular structure, they are easy to twist and aggregate into block structures. The combination of the two can greatly improve the mechanical stability of the superhydrophobic self-healing coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1The synthetic route diagram of DTMS@PDA@SiO2@CNTs composite material;
[0022] Figure 2 Schematic diagram of the EP / DTMS@PDA@SiO2@CNTs superhydrophobic anticorrosion coating;
[0023] Figure 3 The effect of near-infrared light of different power densities on the photothermal conversion performance of DTMS@PDA@SiO2@CNTs prepared at different reaction pH values, where (a) pH = 7.5, (b) pH = 8.5, and (c) pH = 9.5.
[0024] Figure 4 The effect of near-infrared light of different power densities on the photothermal conversion performance of DTMS@PDA@SiO2@CNTs prepared at different reaction temperatures, where (a) the temperature is 20°C, (b) the temperature is 30°C, (c) the temperature is 40°C, and (d) the temperature is 50°C.
[0025] Figure 5 The effect of near-infrared light of different power densities on the photothermal conversion performance of DTMS@PDA@SiO2@CNTs prepared with different CNTs and TEOS addition amounts is shown in Figure 2. 20 @CNTs 40 , (b) Using SiO 240 @CNTs 40 , (c) Using SiO 280 @CNTs 40 , (d) Use SiO 2120 @CNTs 40 , (e) Use SiO 2160 @CNTs 40 ;
[0026] Figure 6 The effect of different power density of near-infrared light on the photothermal conversion performance of DTMS@PDA@SiO2@CNTs prepared with different DA and CNTs addition amounts, where (a) DA:CNTs = 1:2, (b) DA:CNTs = 1:1, (c) DA:CNTs = 2:1;
[0027] Figure 7 This is the wetting process of water droplets on the surface of EP / DTMS@PDA@SiO2@CNTs in Example 5;
[0028] Figure 8 The microstructure of the EP / DTMS@PDA@SiO2@CNTs surface in Example 5;
[0029] Fig. 9 This is the EDS image of EP / DTMS@PDA@SiO2@CNTs in Example 5;
[0030] Fig.10 This is the superhydrophilic process of the EP / DTMS@PDA@SiO2@CNTs surface in Example 6;
[0031] Fig.11 This is a diagram showing the recovery process of the super-hydrophobic properties of the coating before and after etching and irradiation of EP / DTMS@PDA@SiO2@CNTs in Example 6;
[0032] Fig.12 The EDS images of EP / DTMS@PDA@SiO2@CNTs before and after etching-irradiation in Example 6, where (a) is before etching, (b) is after etching, and (c) is after NIR irradiation;
[0033] Fig.13 The surface conditions of EP / DTMS@PDA@SiO2@CNTs during the pressurization-light irradiation process in Example 7, including (a) original coating, (b) after pressurization and deformation, and (c) after NIR irradiation for 10 minutes;
[0034] Fig.14 This is a diagram showing the change in contact angle during the pressurization-light irradiation process of EP / DTMS@PDA@SiO2@CNTs in Example 7;
[0035] Fig.15 This is a schematic diagram of the sand grinding experiment in Example 8;
[0036] Fig.16 The change of contact angle of EP / DTMS@PDA@SiO2@CNTs during the sand grinding experiment in Example 8;
[0037] Fig.17 The surface morphology changes of EP / DTMS@PDA@SiO2@CNTs during the sanding experiment in Example 8, where (a) shows the surface morphology of the composite coating after 0 times, (b) the 10th time, (c) the 16th time and (d) the 35th time, and (e) to (h) are the corresponding enlarged images;
[0038] Fig.18 This is the polarization curve of EP / DTMS@PDA@SiO2@CNTs in Example 9;
[0039] Fig.19 The wetting process of water droplets on the EP / DTMS@PDA@SiO2@CNTs surface (a) and the EP / DTMS@PDA@CNTs surface (b) in Example 10;
[0040] Fig. 20The microstructures of the surfaces of the EP / DTMS@PDA@SiO2@CNTs coating and the EP / DTMS@PDA@CNTs coating in Example 10, wherein (a) is the EP / DTMS@PDA@CNTs coating, and (b) is the EP / DTMS@PDA@SiO2@CNTs composite coating;
[0041] Fig.21 The contact angles of the coatings prepared with different amounts of TEOS and CNTs added in Example 11;
[0042] Fig. 22 is the surface roughness of the EP / DTMS@PDA@SiO2@CNTs composite coating with different mass fractions in Example 12;
[0043] Fig.23 The wetting properties of the surface of the EP / DTMS@PDA@SiO2@CNTs composite coating with different mass fractions in Example 13. DETAILED DESCRIPTION
[0044] The present invention provides a method for preparing a DTMS@PDA@SiO2@CNTs composite material, comprising the following steps:
[0045] dispersing graphitized carboxylated multi-walled carbon nanotubes in water-a first polar organic solvent to obtain a CNTs dispersion;
[0046] Under alkaline conditions, the CNTs dispersion is mixed with tetraethyl silicate to perform an in-situ growth reaction, and nano-SiO2 is in-situ formed on the surface of the graphitized carboxylated multi-walled carbon nanotubes to obtain SiO2@CNTs;
[0047] Providing a weak alkaline solvent; the pH value of the weak alkaline solvent is 7.5 to 9.5, and the weak alkaline solvent includes water and a second polar organic solvent;
[0048] The SiO2@CNTs, the weak alkaline solvent, dopamine and dodecyltrimethylsilane DTMS are mixed to undergo an oxidative self-polymerization-hydrolysis reaction, wherein the dopamine self-polymerizes on the surface of the SiO2@CNTs to form polydopamine PDA, and simultaneously the DTMS is hydrolyzed to generate silanols that are grafted onto the surface of the SiO2@CNTs to obtain a DTMS@PDA@SiO2@CNTs composite material.
[0049] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0050] The invention disperses graphitized carboxylation multi-wall carbon nanotubes in water-a first polar organic solvent to obtain a CNTs dispersion.
[0051] In the present invention, the inner diameter of the graphitized carboxylated multi-walled carbon nanotube is preferably 5-10 nm, the outer diameter is preferably 10-20 μm, the length is preferably 10-30 μm, the purity is >99%, the carboxyl content is about 4 wt%, and it is purchased from McLean Chemical Reagent Co., Ltd. The graphitized carboxylated multi-walled carbon nanotube has a high Young's modulus and tensile strength, which are properties that ordinary single-walled carbon nanotubes do not have. The use of graphitized carboxylated multi-walled carbon nanotubes in the present invention is conducive to improving the mechanical stability of the coating.
[0052] In the present invention, the first polar organic solvent preferably includes one or more of ethanol, methanol, isopropanol, acetone, acetonitrile, dimethyl sulfoxide and N,N-dimethylformamide, and is more preferably ethanol; the volume ratio of the first polar organic solvent to water is preferably 8 to 15:1, and is more preferably 10:1. The concentration of graphitized carboxylated multi-walled carbon nanotubes in the CNTs dispersion is preferably 3 to 4.5 g / L, and is more preferably 4 g / L.
[0053] The present invention has no special requirements for the dispersion process, as long as the graphitized carboxylated multi-walled carbon nanotubes can be evenly dispersed. In the embodiment of the present invention, the dispersion process is specifically performed by ultrasonication in a 55 Hz water bath ultrasonicator for 30 minutes.
[0054] After obtaining the CNTs dispersion, the present invention mixes the CNTs dispersion with tetraethyl silicate under alkaline conditions to carry out an in-situ growth reaction, in-situ forming nano-SiO2 on the surface of the graphitized carboxylated multi-walled carbon nanotubes to obtain SiO2@CNTs.
[0055] The present invention preferably adds tetraethyl silicate (TEOS) to the CNTs dispersion under stirring conditions, and then adjusts the pH value to alkaline conditions to perform an in-situ growth reaction. In the present invention, the mass ratio of the tetraethyl silicate to the mass ratio of the graphitized carboxylated multi-walled carbon nanotubes in the CNTs dispersion is preferably 3 to 4:1, more preferably 3:1; the pH value of the alkaline conditions is preferably 8 to 10; the present invention preferably uses sodium hydroxide solution, potassium hydroxide solution, ammonia water, sodium carbonate solution or sodium bicarbonate solution to adjust the pH value.
[0056] In the present invention, the in-situ growth reaction is preferably carried out at room temperature, that is, no additional heating or cooling is required, and the time of the in-situ growth reaction is preferably 8 to 24 hours, more preferably 12 to 16 hours. Tetraethyl silicate contains a coupling group (-Si-), which reacts with the carboxyl group on the surface of the carboxylated carbon nanotubes under alkaline conditions to grow nano-SiO2 on the surface of CNTs in situ. SiO2 is highly wear-resistant; the SiO2 formed at the same time causes gaps between CNTs, which are not easy to agglomerate; SiO2 and CNTs jointly construct a micro-nano structure on the coating surface.
[0057] After the in-situ growth reaction is completed, the present invention preferably further comprises washing the obtained mixture to neutrality and drying to obtain SiO2@CNTs.
[0058] The present invention provides a weak alkaline solvent; the pH value of the weak alkaline solvent is 7.5-9.5, preferably 8.5; the weak alkaline solvent comprises water and a second polar organic solvent.
[0059] In the present invention, the second polar organic solvent preferably includes N,N-dimethylformamide, acetone, acetonitrile or dimethyl sulfoxide, more preferably N,N-dimethylformamide; the volume ratio of water to the second polar organic solvent is preferably 1:4.
[0060] In the present invention, water and a second polar organic solvent are preferably mixed, and then an alkali solution is added to adjust the pH value to 8 to 9.5. The alkali solution preferably includes sodium hydroxide solution, potassium hydroxide solution, ammonia water, sodium carbonate solution or sodium bicarbonate solution.
[0061] After obtaining SiO2@CNTs and a weakly alkaline solvent, the present invention mixes the SiO2@CNTs, the weakly alkaline solvent, dopamine and dodecyltrimethylsilane (DTMS) to carry out an oxidative self-polymerization-hydrolysis reaction to obtain a DTMS@PDA@SiO2@CNTs composite material.
[0062] In the present invention, the mass ratio of the dopamine to the graphitized carboxylated multi-walled carbon nanotubes is preferably 0.5 to 2:1, more preferably 1 to 1.5:1; the mass ratio of the DTMS to dopamine is preferably 1 to 3:10, more preferably 1 to 2:10; the temperature of the oxidative self-polymerization-hydrolysis reaction is preferably 20 to 50°C, more preferably 30 to 50°C, most preferably 40°C, and the time is preferably 12 to 24h, more preferably 12 to 18h.
[0063] In the present invention, mixing the SiO2@CNTs, the weak alkaline solvent, dopamine and dodecyltrimethylsilane (DTMS) preferably includes: first dispersing the SiO2@CNTs in a weak alkaline solvent, then heating the resulting dispersion to a temperature for an oxidative self-polymerization-hydrolysis reaction, and adding dopamine and DTMS to the reaction system.
[0064] In the present invention, the concentration of SiO2@CNTs in the weak alkaline solvent is preferably 60-80 g / L, more preferably 65-75 g / L. In the present invention, SiO2@CNTs are preferably added to the weak alkaline solvent and stirred and ultrasonicated for 30 minutes to achieve uniform dispersion.
[0065] Under weak alkaline conditions, dopamine (DA) can undergo oxidative self-polymerization on the surface of SiO2 and CNTs to form a PDA coating, and further generate a PDA@SiO2@CNTs complex rich in amino and catechol groups. The improved PDA coating not only functions as a binder, but also enhances the interfacial adhesion between SiO2 and CNTs. In addition, it can also give carbon nanomaterials chemical activity, thereby improving the photothermal properties of these materials and providing them with a platform for secondary reactions.
[0066] The methoxyl group (-OCH3) in DTMS reacts with water (H2O) to generate silanol (-Si-OH) and methanol (CH3OH), which condenses with the carboxyl group (-COOH) on the surface of the carbon nanotubes to be grafted onto SiO2@CNTs. The aliphatic chain with lower surface energy can modify the surface of the carbon nanomaterial through hydrogen bonding, thereby ultimately reducing the surface energy of the coating.
[0067] After the oxidative self-polymerization-hydrolysis reaction is completed, the present invention centrifuges, washes, and dries the obtained product liquid to obtain a DTMS@PDA@SiO2@CNTs composite material.
[0068] In the present invention, the synthesis path of the DTMS@PDA@SiO2@CNTs composite material is as follows: Figure 1 shown.
[0069] The present invention provides a DTMS@PDA@SiO2@CNTs composite material prepared by the preparation method described in the above scheme, comprising SiO2@CNTs, PDA located on the surface of the SiO2@CNTs, and silanol chains grafted on the SiO2@CNTs; the silanol chains are obtained by hydrolysis of DTMS; the SiO2@CNTs comprise graphitized carboxylated multi-walled carbon nanotubes and nano-SiO2 in-situ grown on the surface of the graphitized carboxylated multi-walled carbon nanotubes.
[0070] The present invention provides application of the DTMS@PDA@SiO2@CNTs composite material in a super-hydrophobic coating.
[0071] The present invention provides a super-hydrophobic self-repairing anti-corrosion coating, comprising epoxy resin, the above-mentioned DTMS@PDA@SiO2@CNTs composite material, a curing agent and an organic solvent.
[0072] In the present invention, the epoxy resin is preferably E-51 epoxy resin; the curing agent is preferably D203 curing agent. The present invention does not specifically limit the usage relationship of the epoxy resin and the curing agent, and the ratio well known in the art can be used to ensure that the epoxy resin is cured.
[0073] In the present invention, the mass of the DTMS@PDA@SiO2@CNTs composite material is preferably 15-35% of the total mass of the epoxy resin, the curing agent and the DTMS@PDA@SiO2@CNTs composite material, and more preferably 20-30%.
[0074] In the present invention, the organic solvent is preferably ethanol. The present invention does not make special requirements on the amount of the organic solvent, and a suitable amount can be selected according to the coating method of the coating, which is common knowledge in the art. In an embodiment of the present invention, the coating method is spraying, and the mass of the organic solvent is 5 times that of the epoxy resin.
[0075] The present invention has no special requirements for the preparation method of the super-hydrophobic self-repairing anti-corrosion coating, as long as the components can be mixed evenly.
[0076] The invention provides a super-hydrophobic self-repairing anti-corrosion coating, comprising an epoxy resin and a DTMS@PDA@SiO2@CNTs composite material embedded in the epoxy resin.
[0077] In the present invention, the mass of the DTMS@PDA@SiO2@CNTs composite material is preferably 15-35% of the mass of the epoxy resin (including the curing agent), and more preferably 20-30%.
[0078] The super-hydrophobic self-repairing anti-corrosion coating provided by the present invention has near-infrared light responsive shape memory properties. After being irradiated with near-infrared light, the temperature of the coating can rise rapidly, and the super-hydrophobic property can be quickly restored after the micro-nano structure on the coating surface is destroyed or the surface energy is increased, resulting in the loss of super-hydrophobic property.
[0079] The present invention provides a method for preparing the super-hydrophobic self-repairing anti-corrosion coating described in the above scheme, comprising the following steps: applying the super-hydrophobic self-repairing anti-corrosion coating described in the above scheme to the surface of a metal substrate, and curing to obtain the super-hydrophobic self-repairing anti-corrosion coating.
[0080] The present invention has no special requirements on the material of the metal substrate, and any metal substrate well known to those skilled in the art may be used, such as a steel substrate.
[0081] Before the coating, the present invention preferably pre-treats the metal substrate; the pre-treatment preferably includes grinding, cleaning, alkali cleaning and pickling in sequence; before the grinding, the present invention preferably first rinses the metal substrate with deionized water, degreases with acetone, dehydrates with anhydrous ethanol, and then blows it dry for standby use. In the present invention, the grinding is preferably to use 180#, 400#, 600#, 800#, 1200# sandpaper to grind the metal substrate in sequence; the cleaning is preferably to first clean the metal surface debris with deionized water, and then use acetone and anhydrous ethanol for ultrasonic cleaning in sequence, and the time for ultrasonic cleaning with acetone and ultrasonic cleaning with anhydrous ethanol is preferably 3 to 5 minutes independently.
[0082] In the present invention, the solute of the alkaline washing solution for alkaline washing is preferably sodium hydroxide, sodium carbonate and sodium silicate, and the solvent is preferably water; the concentration of sodium hydroxide in the alkaline washing solution is preferably 12g / L, the concentration of sodium carbonate is preferably 60g / L, and the concentration of sodium silicate is preferably 30g / L; the temperature of the alkaline washing is preferably 75°C, and the time is preferably 10min. The present invention removes oil through alkaline washing, and can also wash away metal debris, scum, abrasives, carbon residue, etc.
[0083] In the present invention, the acid used for pickling is preferably dilute hydrochloric acid with a mass fraction of 10%, and the pickling time is preferably 1 minute; the present invention activates the metal substrate by pickling.
[0084] In the present invention, the coating is preferably spraying, the nozzle diameter is preferably 0.8 mm, the compressed air pressure is preferably 0.3 MPa, and the spraying distance is preferably 14 to 17 cm.
[0085] In the present invention, the curing is preferably room temperature curing.
[0086] The DTMS@PDA@SiO2@CNTs composite material provided by the present invention and its preparation and application, super hydrophobic self-healing anti-corrosion coating, coating and its preparation are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0087] Example 1
[0088] In the DTMS@PDA@SiO2@CNTs particle preparation process, the initial pH value of the reaction system is directly related to the progress of DA self-oxidation polymerization, thereby affecting the grafting efficiency of the reaction. The initial pH of the reaction (i.e., the pH of the weakly alkaline solvent) was set to 7.5, 8.5, and 9.5 to prepare DTMS@PDA@SiO2@CNTs. The temperature changes of the reaction product preparation solution at each initial pH are shown in Figure 2. Figure 3 As shown, (a) is pH = 7.5, (b) is pH = 8.5, and (c) is pH = 9.5.
[0089] Preparation process of reaction product solution:
[0090] (1) 8 mg of graphitized carboxylated multi-walled carbon nanotubes (c-CNTs) were dispersed in 20 mL of anhydrous ethanol / distilled water (volume ratio of 10:1) solution and sonicated in a 55 Hz water bath sonicator for 30 min to uniformly disperse the carbon nanotubes in the solution;
[0091] (2) Under magnetic stirring, 24 mg of tetraethyl silicate (TEOS) was added to the mixture, and NaOH solution was added to a pH of 8. After reacting for 12 hours, the mixture was washed to a neutral pH and dried at 80°C to obtain SiO2@CNTs;
[0092] (3) 5 mL of deionized water was mixed with 20 mL of N,N-dimethylformamide (DMF) and the pH was adjusted to 7.5, 8.5 and 9.5 with the prepared sodium hydroxide solution. SiO2@CNTs were added to the solution and stirred and ultrasonicated for 30 minutes, and the temperature was heated to 40°C. 8 mg of dopamine hydrochloride (DA) and 0.1 mL of dodecyltrimethylsilane were added and stirred for 24 h.
[0093] (4) After the reaction, DTMS@PDA@SiO2@CNTs were obtained after centrifugation (1000 rpm, 10 min), washing with deionized water, and drying (80°C, 12 h).
[0094] Under different irradiation powers, when the pH is 7.5, the temperature changes of 10 minutes at three irradiation powers are 9.1℃, 13.4℃ and 16.2℃ respectively; when the reaction pH is 8.5, the temperature changes of the reaction product solution at three irradiation powers for 10 minutes are 11.6℃, 17.8℃ and 23.9℃; when the reaction pH is 9.5, the temperature changes of the reaction product solution at three irradiation powers for 10 minutes are 8.3℃, 14.1℃ and 16.1℃. The results show that the synthesized DTMS@PDA@SiO2@CNTs particles have a certain photothermal conversion ability, and the photothermal conversion ability of the particles is the strongest when the pH is 8.5. Therefore, the initial pH of the reaction is 8.5 for subsequent experiments.
[0095] Example 2
[0096] The pH was set to 8.5, and the water bath temperature (i.e., DA oxidation self-polymerization temperature) was set to 20°C, 30°C, 40°C, and 50°C to prepare DTMS@PDA@SiO2@CNTs. Other conditions were the same as in Example 1. The temperature changes of the reaction product solution at each reaction temperature are shown in FIG. Figure 4As shown, (a) the temperature is 20°C, (b) the temperature is 30°C, (c) the temperature is 40°C, and (d) the temperature is 50°C. Under different irradiation powers, when the reaction temperature is 20°C, the temperature changes of the reaction product solution under three irradiation power densities are: 6.1°C, 7.9°C, 11.2°C; when the reaction temperature is 30°C, the temperature changes of the reaction product solution under three irradiation power densities are: 8.6°C, 10.3°C, 15.8°C; when the reaction temperature is 40°C, the temperature changes of the reaction product solution under three irradiation power densities are: 12.9°C, 16.4°C, 21.1°C; when the reaction temperature is 50°C, the temperature changes of the reaction product solution under three irradiation power densities are: 12.6°C, 15.9°C, 19.8°C. When the reaction temperature is 40°C, the photothermal conversion capacity is the best.
[0097] Example 3
[0098] CNTs have rich conjugated structures inside the molecule, have strong light absorption in the visible-near infrared region, and produce significant photothermal effects through molecular thermal vibrations. When the added CNTs:TEOS is too large, the CNTs themselves become entangled, which is not conducive to the photothermal conversion performance of the particles. When the added CNTs:TEOS is too small, there are too many SiO2 nanoparticles attached to the surface of the CNTs, and the photothermal conversion ability of the particles decreases.
[0099] In order to further explore the optimal addition amount of CNTs and TEOS, the pH was set to 8.5, the mass of CNTs was set to 40 mg, and the addition amount of TEOS was 0, 40 mg, 80 mg, 120 mg, and 160 mg respectively. The obtained particles were recorded as SiO 20 @CNTs 40 、SiO 240 @CNTs 40 、SiO 280 @CNTs 40 、SiO 2120 @CNTs 40 、SiO 2160 @CNTs 40 . PDA was mixed with SiO 20 @CNTs 40 、SiO 240 @CNTs 40 (the mass ratio of CNTs and TEOS is 1:1), SiO 280 @CNTs 40 (the mass ratio of CNTs and TEOS is 1:2), SiO 2120 @CNTs 40 (the mass ratio of CNTs and TEOS is 1:3), SiO2160 @CNTs 40 (the mass ratio of CNTs to TEOS is 1:4) and the other conditions are the same as in Example 1. The temperature of the solution prepared by the reaction product with different addition amounts is as follows Figure 5 As shown, (a) using SiO 20 @CNTs 40 , (b) Using SiO 240 @CNTs 40 , (c) Using SiO 280 @CNTs 40 , (d) Use SiO 2120 @CNTs 40 , (e) Use SiO 2160 @CNTs 40 PDA modified SiO under different irradiation powers 20 @CNTs 40 The temperature changes of the reaction product solutions were: 4.3℃, 5.2℃, 6.5℃; PDA modified SiO 240 @CNTs 40 The temperature changes of the reaction product solutions were 5.5℃, 6.6℃, and 8.9℃ respectively; 280 @CNTs 40 The temperature changes of the reaction product solutions were: 6.9℃, 9.6℃, 15.8℃; PDA modified SiO 2120 @CNTs 40 The temperature changes of the reaction product solutions were: 8.2℃, 14.2℃, 24.1℃; PDA modified SiO 2160 @CNTs 40 The temperature changes of the reaction product solution are: 7.9℃, 13.6℃, 22.6℃. 2120 @CNTs 40 When the mass ratio of CNTs to TEOS is 1:3-4, the photothermal conversion capacity is better, and 1:3 is the best. Therefore, the subsequent experiments were carried out with a mass ratio of CNTs to TEOS of 1:3.
[0100] Example 4
[0101] In order to further explore the optimal addition amount of DA, the pH was set to 8.5, and the ratio of DA to CNTs was set to 1:2, 1:1, and 2:1, respectively. The other conditions were the same as in Example 1. The temperature of the reaction product solution under different DA addition amounts was as follows: Figure 6As shown, (a) DA:CNTs = 1:2, (b) DA:CNTs = 1:1, (c) DA:CNTs = 2:1. Under different irradiation powers, the temperature changes of the reaction product solution after the ratio of DA to CNTs is 1:2 are 6.8℃, 13.6℃, 21.4℃ respectively; the temperature changes of the reaction product solution after the ratio of DA to CNTs is 1:1 are 8.3℃, 16.1℃, 25.1℃ respectively; the temperature changes of the reaction product solution after the ratio of DA to CNTs is 2:1 are 7.2℃, 14.9℃, 23.6℃ respectively. When the ratio of DA to CNTs is 1:1, the photothermal conversion ability of the particles is the strongest.
[0102] Example 5
[0103] 20# carbon steel was selected as the metal substrate with a size of 50mm×25mm×2mm. After being rinsed with deionized water, it was degreased with acetone and dehydrated with anhydrous ethanol, and dried with a cold air blower for use.
[0104] S1: First, pre-treat the metal substrate, the steps are as follows:
[0105] (1) Grinding the metal substrate with 180#, 400#, 600#, 800#, and 1200# sandpaper in sequence, cleaning the metal surface debris with deionized water, and then ultrasonically cleaning the substrate with acetone and anhydrous ethanol solution for 3 to 5 minutes respectively, and drying with a cold air blower for later use;
[0106] (2) preparing an alkaline cleaning solution, wherein the alkaline cleaning solution is composed of sodium hydroxide, sodium carbonate, sodium silicate and water, wherein the concentration of sodium hydroxide is 12 g / L, the concentration of sodium carbonate is 60 g / L, and the concentration of sodium silicate is 30 g / L, and then alkaline cleaning is performed on the metal substrate at a constant temperature of 75° C. for 10 min;
[0107] (3) Activate the metal substrate with 10 wt % dilute hydrochloric acid for 1 min.
[0108] S2: Prepare DTMS@PDA@SiO2@CNTs mixed solution, the steps are as follows:
[0109] (1) 8 mg of graphitized carboxylated multi-walled carbon nanotubes (c-CNTs) were dispersed in 20 mL of anhydrous ethanol / distilled water (volume ratio of 10:1) solution and sonicated in a 55 Hz water bath sonicator for 30 min to uniformly disperse the carbon nanotubes in the solution;
[0110] (2) Under magnetic stirring, 24 mg of tetraethyl silicate (TEOS) was added to the mixture, and NaOH solution was added to a pH of 8. After reacting for 12 hours, the mixture was washed to a neutral pH and dried at 80°C to obtain SiO2@CNTs;
[0111] (3) Mix 20 mL of N,N-dimethylformamide (DMF) with 5 mL of deionized water and adjust the pH to 8.5 with the prepared sodium hydroxide solution. Add SiO2@CNTs to the solution and stir and sonicate for 30 minutes, then heat the temperature to 40°C. Add 8 mg of dopamine hydrochloride (DA) and 0.1 mL of dodecyltrimethylsilane and stir for 24 hours.
[0112] (4) After the reaction, DTMS@PDA@SiO2@CNTs were obtained after centrifugation (1000 rpm, 10 min), washing with deionized water, and drying (80°C, 12 h).
[0113] S3: Preparation of EP / DTMS@PDA@SiO2@CNTs super-hydrophobic self-healing anti-corrosion coating by one-step spraying method, the steps are as follows:
[0114] (1) At room temperature, E-51 epoxy resin and D203 curing agent were uniformly mixed in a ratio of 1:1, and then 30 wt% of DTMS@PDA@SiO2@CNTs were added. Anhydrous ethanol was added and stirred, and ultrasonication was performed for 5 minutes to make the suspension uniformly dispersed.
[0115] (2) Use a spray gun to evenly spray the suspension onto the base metal, wherein the nozzle diameter is 0.8 mm, the compressed air pressure is 0.3 MPa, the spraying distance is about 15 cm, and the coating thickness is about 120 μm.
[0116] After the EP / DTMS@PDA@SiO2@CNTs composite coating was dried at room temperature for two weeks, the wettability of the coating was tested and its static hydrophobic angle could reach 167° (e.g. Figure 7 shown).
[0117] The SEM images of the obtained EP / DTMS@PDA@SiO2@CNTs super hydrophobic anti-corrosion coating at different magnifications are shown in Figure 2. Figure 8 As shown, the magnification of (a) is 10000, and the magnification of (b) is 50000. Figure 8 It can be seen that the epoxy-coated DTMS@PDA@SiO2@CNTs particles construct a well-defined rough structure on the coating surface. A large number of nano-sized SiO2@CNTs particles are attached to the surface of these microsphere clusters, and the composite coating successfully constructs a peak microstructure and a fuzzy nanostructure. These particles aggregate to varying degrees on the coating surface, significantly improving the roughness of the coating surface and playing a key role in the superhydrophobic properties of the coating.
[0118] EDS image of EP / DTMS@PDA@SiO2@CNTs super hydrophobic self-healing anti-corrosion coating Fig. 9As shown. Among them, C and O elements mainly come from epoxy resin and SiO2, N element mainly comes from PDA, and Si element mainly comes from SiO2 and DTMS. The mass proportion of the characteristic element C of the coating is 57.82wt%, N element is 1.97wt%, O element is 25.75wt%, and Si element is 14.46wt%. It was detected that Si and N elements successfully entered the epoxy system, while C element was still the highest, proving that epoxy resin is still the main component of the composite coating.
[0119] Example 6
[0120] The preparation method of the EP / DTMS@PDA@SiO2@CNTs super hydrophobic self-healing anti-corrosion coating is consistent with that in Example 5, and its low surface energy self-healing performance is tested.
[0121] Superhydrophobicity can be restored by low surface energy substances migrating to the surface, provided that the microscopic morphology remains intact or is not severely damaged. There are a large number of polar groups on the superhydrophobic surface, which reduces the surface energy of the composite coating. In practical applications, these polar groups may be oxidized by oxygen and oxides in the air, resulting in the loss of low surface energy on the surface of the composite coating. Oxidation and decomposition in nature are very slow, and oxygen plasma etching is usually used to simulate the situation of superhydrophobic coatings after long-term oxidation and decomposition damage.
[0122] like Fig.10 As shown, after the composite coating is etched, the water droplets quickly penetrate into the coating. At this time, the composite coating has completely lost its hydrophobic properties, and the static contact angle is 0°, where (a) is 0ms, (b) is 6ms, and (c) is 12ms.
[0123] The composite coating after O2 plasma etching was irradiated under NIR for 10 minutes, and the contact angle change of the composite coating was measured after the coating was cooled to room temperature again. Thanks to the excellent photothermal conversion performance of the composite coating, the super-hydrophobicity of the composite coating was quickly restored under near-infrared light after being irradiated with near-infrared light. Fig.11 The super-hydrophilic state of the composite coating is shown in Figure 2. The wavelength is 808nm and the power density is 2w / cm at a distance of 20cm. 2 After irradiation with near-infrared light for 10 minutes, the surface regained its superhydrophobicity and the contact angle recovered from 0° to about 160°.
[0124] EDS testing was used to characterize the chemical composition of the composite coating before and after repair. Fig.12As shown, (a) is before etching, (b) is after etching, and (c) is after NIR irradiation. The O content in the composite coating increased from 24.44wt% before etching to 35.99wt% after etching. After NIR irradiation, the O content decreased to 27.87wt%, which is not much different from the O content before etching. Combined with the above analysis, this transition from superhydrophobicity to superhydrophilicity is due to the presence of a large number of polar oxygen-containing groups (such as -OH) on the surface of the coating. Due to the high surface energy of the coating surface at this time, it is thermodynamically unstable. Under the irradiation of near-infrared light, the low surface energy substance DTMS@PDA@SiO2@CNTs in the composite coating migrates in the direction of light, causing the surface energy of the composite coating to decrease again, restoring its superhydrophobic properties.
[0125] Example 7
[0126] The preparation method of the EP / DTMS@PDA@SiO2@CNTs super-hydrophobic self-healing anti-corrosion coating is consistent with that in Example 5, and its micro-nano structure self-healing performance is tested.
[0127] The micro-nano structure of the super-hydrophobic surface is easily damaged by external forces, and the micro-nano structure of the coating surface can be restored through the movement of molecular chains. A tablet press is used to simulate the damage of the micro-nano structure on the surface of the composite coating, and to explore the self-repair performance and super-hydrophobic recovery performance of the surface micro-nano structure of the composite coating. Fig.13 (a) to (c) show the 3D morphology of the original coating, the coating after pressure deformation (the right half is the pressure-bearing coating), and the coating after NIR irradiation for 10 minutes.
[0128] It can be seen that the original coating has an obvious micro-nano structure on the surface, and spherical clusters are evenly distributed on the surface. After pressurization, there are obvious flat indentations on the coating surface, the surface microstructure is destroyed, and the spherical clusters are squeezed into granules. After irradiation under NIR for 10 minutes, the micro-nano structure of the coating surface is restored, and the spherical clusters can be clearly observed again.
[0129] like Fig.14As shown, the change in the wetting properties of the coating before and after compression is intuitively demonstrated. In the uncompressed state, the water contact angle of the EP / DTMS@PDA@SiO2@CNTs composite coating is as high as 167.59°, reflecting its excellent superhydrophobic properties. However, when the coating is subjected to external pressure, the micro-nano structure on its surface is damaged, and the static contact angle of the coating drops significantly to 135.42°, indicating that the coating has lost its superhydrophobic properties. This is because the micro-nano structure on the surface of the coating is flattened due to pressure, which increases the contact area between the liquid and the solid part of the coating surface, thereby reducing the hydrophobic properties of the coating and enhancing the adhesion of water droplets on the coating surface. After the compressed EP / DTMS@PDA@SiO2@CNTs composite coating was irradiated under NIR for 10 minutes, the contact angle of the coating rose to 165.01°, and the coating surface restored its hydrophobic properties.
[0130] Example 8
[0131] Improving the mechanical stability (wear resistance) of the super-hydrophobic coating is one of the purposes of the present invention. In this embodiment, the mechanical stability of the EP / DTMS@PDA@SiO2@CNTs super-hydrophobic self-repairing anti-corrosion coating is tested by a sanding experiment. The preparation method of the EP / DTMS@PDA@SiO2@CNTs super-hydrophobic self-repairing anti-corrosion coating is the same as that in Example 5.
[0132] The test process is as follows: Place the coating surface facing downward on 400# sandpaper, place a 100g weight on the sample to apply a certain pressure to the coating, drag the sample on the sandpaper surface at a constant speed of 1.6cm / s, and measure the change in the contact angle of the coating surface within different wear distances to characterize the wear resistance of the coating. The schematic diagram of the test process is shown in the figure Fig.15 shown.
[0133] Fig.16 The contact angle changes of the EP / DTMS@PDA@SiO2@CNTs composite coating after different wear distances are shown. It can be seen from the figure that the original contact angle of the composite coating is 167.52°. When the sanding distance is small, the contact angle of the coating surface does not change significantly. When the wear exceeds 4 times, the contact angle of the coating decreases to a certain extent. At this time, the contact angle is 161.59°. When the wear number reaches 5 times, the contact angle becomes 162.24°. The coating surface continues to be sanded. When the wear number reaches 15 times, the contact angle drops to 158.22°. When the wear number is 16 times, the contact angle rises to 160.23°. When the wear number reaches 25 times, the contact angle of the coating still reaches 156.12°, and the superhydrophobic property of the coating can still be well maintained. When the wear number reaches 34, the contact angle of the composite coating decreases to 151.99°, indicating that the composite coating has excellent mechanical stability.
[0134] according to Fig.16 After the composite coating was worn for the 5th, 7th, 9th, 10th, 16th, 19th, 24th, 28th and 31st times, the contact angle of the coating was improved to varying degrees. In order to further explore the damage mechanism of sandpaper on the coating, the surface morphology of the coating after 4 times of sandpaper wear was tested. Fig.17 As shown, (a) shows the surface morphology of the composite coating after 0 times, (b) the 10th time, (c) the 16th time and (d) the 35th time, and (e) to (h) are the corresponding enlarged images. Under the abrasive action of sandpaper, the original layered structure of the coating surface is destroyed. Compared with the coating before wear, the height of the peak protrusions is greatly reduced, and the coating becomes flatter. In summary, during the continuous wear process, the constructed special micro-nano structure is constantly destroyed, resulting in a slight decrease in the superhydrophobicity of the coating surface.
[0135] In the sandpaper wear experiment, the strong cohesion and interfacial adhesion exhibited by the composite coating are mainly attributed to the following two aspects: First, the highly cross-linked EP in the coating can firmly bind the carbon nanomaterials together. In the high-magnification SEM image, although the surface of the peak-like structure was polished smooth, SiO2 and CNTs were still tightly bound, which was attributed to the bonding effect of PDA. Secondly, CNTs not only have a high Young's modulus and tensile strength, but also are easy to twist and aggregate into block structures due to their one-dimensional tubular structure. Specifically, after the 5th, 7th, 9th, 10th, 16th, 19th, 24th, 28th and 31st wear, the WCA of the coating showed different degrees of improvement, as if the superhydrophobic surface of the coating was self-healing. By observing Fig.17 It can be seen that after the surface was worn, the newly exposed SiO2@CNTs reconstructed a new rough structure in the presence of PDA and EP, which plays a crucial role in maintaining the superhydrophobic property after wear damage.
[0136] Example 9
[0137] Corrosion is considered to be a key factor leading to metal damage, and the core goal of coating protection is to curb the generation and expansion of metal corrosion. Before the smart coating is officially put into production and application, it is extremely critical to conduct a comprehensive evaluation and investigation of its anti-corrosion properties. In addition, in the application of epoxy-based coatings, the addition of DTMS@PDA@SiO2@CNTs particles introduces a new type of medium particles into the coating, which will undoubtedly have a certain degree of influence on the anti-corrosion properties of the coating. The preparation method of EP / DTMS@PDA@SiO2@CNTs superhydrophobic self-healing anti-corrosion coating is the same as that in Example 5.
[0138] A bare carbon steel substrate and a carbon steel substrate coated with an ordinary epoxy resin coating were used as comparisons, wherein the thickness of the ordinary epoxy resin coating was consistent with the thickness of the EP / DTMS@PDA@SiO2@CNTs superhydrophobic anti-corrosion coating.
[0139] The method for corrosion resistance test is as follows: a standard three-electrode system is used, with a bare carbon steel substrate, a carbon steel substrate coated with an ordinary epoxy resin coating, and a carbon steel substrate sprayed with an EP / DTMS@PDA@SiO2@CNTs super-hydrophobic self-repairing anti-corrosion coating as working electrodes, a saturated calomel electrode and a platinum electrode as reference electrodes and auxiliary electrodes, and the corrosive medium is a 3.5% by mass NaCl aqueous solution, and a polarization curve test is carried out.
[0140] The polarization curve test results are as follows: Fig.18 As shown, the corrosion potential and corrosion current density of each sample were obtained by fitting the polarization curve. The anti-corrosion efficiency η of the coating was calculated according to formula (1). The obtained data are shown in Table 1.
[0141] The polarization curve test results obtained by formula (1) are as follows Fig.18 As shown, the corrosion potential and corrosion current density of each sample were obtained by fitting the polarization curve. The anti-corrosion efficiency η of the coating was calculated according to formula (1). The obtained data are shown in Table 1.
[0142]
[0143] In formula (1), icorr,sub and icorr,coated are the corrosion current densities of the bare substrate and the coated substrate, respectively.
[0144] Table 1 Polarization curve fitting data
[0145] sample Ecorr / mV <![CDATA[icorr / A·cm -2 ]]> η Carbon steel substrate -584 8.69×10-6 —— Epoxy resin -421 4.35×10-6 49.94% Composite coating -398 4.24×10-7 95.12%
[0146] Compared with bare carbon steel, the sample coated with pure epoxy resin coating has obvious positive shift of corrosion potential, slightly reduced corrosion current density, and calculated anti-corrosion efficiency of about 49.94%; the corrosion potential of EP / DTMS@PDA@SiO2@CNTs composite coating with super hydrophobicity is the smallest, the corrosion current density is 1 / 20 of bare steel and 1 / 10 of pure epoxy coating, and the anti-corrosion efficiency is as high as 95.12%. It shows that the anti-corrosion performance of the composite coating is significantly higher than that of epoxy coating, and it plays a good protective role on the metal substrate.
[0147] Example 10
[0148] The amount of TEOS added will affect the morphology of SiO2 on the surface of CNTs and the hydrophobicity of the coating. The present invention prepared EP / DTMS@PDA@SiO2@CNTs composite coating and EP / DTMS@PDA@CNTs coating for comparison.
[0149] 20# carbon steel was selected as the metal substrate with a size of 50mm×25mm×2mm. After being rinsed with deionized water, it was degreased with acetone and dehydrated with anhydrous ethanol, and dried with a cold air blower for use.
[0150] S1: First, pre-treat the metal substrate, the steps are as follows:
[0151] (1) Grinding the metal substrate with 180#, 400#, 600#, 800#, and 1200# sandpaper in sequence, cleaning the metal surface debris with deionized water, and then ultrasonically cleaning the substrate with acetone and anhydrous ethanol solution for 3 to 5 minutes respectively, and drying with a cold air blower for later use;
[0152] (2) preparing an alkaline cleaning solution, wherein the alkaline cleaning solution is composed of sodium hydroxide, sodium carbonate, sodium silicate and water, wherein the concentration of sodium hydroxide is 12 g / L, the concentration of sodium carbonate is 60 g / L, and the concentration of sodium silicate is 30 g / L, and then alkaline cleaning is performed on the metal substrate at a constant temperature of 75° C. for 10 min;
[0153] (3) Activate the metal substrate with 10 wt % dilute hydrochloric acid for 1 min.
[0154] S2: Prepare a mixed solution of DTMS@PDA@SiO2@CNTs and DTMS@PDA@CNTs, the steps are as follows:
[0155] (1) 8 mg of graphitized carboxylated multi-walled carbon nanotubes (c-CNTs) were dispersed in 20 mL of anhydrous ethanol / distilled water (volume ratio of 10:1) solution and sonicated in a 55 Hz water bath sonicator for 30 min to uniformly disperse the carbon nanotubes in the solution;
[0156] (2) Under magnetic stirring, 24 mg and 0 mg of tetraethyl silicate (TEOS) were added to the mixture, respectively, and NaOH solution was added to a pH of 8. After reacting for 12 hours, the mixture was washed to a neutral pH and dried at 80 °C to obtain SiO2@CNTs and pure CNTs, respectively;
[0157] (3) 5 mL of deionized water was mixed with 20 mL of N, N-dimethylformamide (DMF) and the pH was adjusted to 8.5 with the prepared sodium hydroxide solution. SiO2@CNTs and pure CNTs were added to the solution and stirred and ultrasonicated for 30 minutes, and the temperature was heated to 40°C. 8 mg of dopamine hydrochloride (DA) and 0.1 mL of dodecyltrimethylsilane were added and stirred for 24 h.
[0158] (4) After the reaction, DTMS@PDA@SiO2@CNTs and DTMS@PDA@CNTs were obtained after centrifugation (1000 rpm, 10 min), washing with deionized water, and drying (80°C, 12 h).
[0159] S3: Preparation of EP / DTMS@PDA@SiO2@CNTs superhydrophobic self-repairing anti-corrosion coating and EP / DTMS@PDA@CNTs coating by one-step spraying method, the steps are as follows:
[0160] (1) At room temperature, E-51 epoxy resin and D203 curing agent were uniformly mixed in a ratio of 1:1, and then 30 wt% of DTMS@PDA@SiO2@CNTs and 30 wt% of DTMS@PDA@CNTs were added respectively, and anhydrous ethanol was added for stirring, and ultrasonication was performed for 5 minutes to make the suspension uniformly dispersed.
[0161] (2) Use a spray gun to evenly spray the suspension onto the base metal. The nozzle diameter is 0.8 mm, the compressed air pressure is 0.3 MPa, the spraying distance is about 15 cm, and the coating thickness is about 120 μm. EP / DTMS@PDA@SiO2@CNTs coating and EP / DTMS@PDA@CNTs coating were successfully prepared.
[0162] After the EP / DTMS@PDA@SiO2@CNTs composite coating and EP / DTMS@PDA@CNTs coating were dried at room temperature for two weeks, the wetting properties of the coatings were tested. The static hydrophobic angle of the EP / DTMS@PDA@SiO2@CNTs composite coating could reach 167°, while the static hydrophobic angle of the EP / DTMS@PDA@CNTs coating was only 123°, which could not reach a superhydrophobic state.
[0163] Fig.19 (a) and (b) show the wetting states of the prepared EP / DTMS@PDA@CNTs composite coating and EP / DTMS@PDA@SiO2@CNTs coating, respectively.
[0164] The SEM images of EP / DTMS@PDA@SiO2@CNTs composite coating and EP / DTMS@PDA@CNTs coating at 2,000 times magnification are shown in Figure 2. Fig. 20As shown, (a) is EP / DTMS@PDA@CNTs coating, and (b) is EP / DTMS@PDA@SiO2@CNTs composite coating. It can be seen that the surface of EP / DTMS@PDA@CNTs coating without TEOS is relatively smooth, without obvious rough structure. The surface of EP / DTMS@PDA@SiO2@CNTs composite coating with TEOS is covered by numerous micron-sized DTMS@PDA@SiO2@CNTs particles, forming a rough appearance of particle aggregation.
[0165] CNTs particles are one-dimensional tubular structures with smooth surfaces. By in-situ growing SiO2 on the surface of CNTs, SiO2@CNTs particles will produce a rough structure, which has greater advantages in constructing superhydrophobic surfaces. In addition, through the entanglement of long carbon nanotubes, SiO2 particles form a three-dimensional network structure. Due to the addition of CNTs and SiO2@CNTs particles, the surface of the composite coating becomes rough. However, the spontaneous aggregation of CNTs particles hinders the adhesion of epoxy resin and forms a loose porous structure. In contrast, SiO2 improves the surface structure of CNTs, thereby enhancing the bonding between particles and EP.
[0166] Embodiment 11
[0167] The mass of CNTs was set to 40 mg, and the addition amounts of TEOS were 0, 40 mg, 80 mg, 120 mg, and 160 mg, respectively. The obtained particles were recorded as SiO 20 @CNTs 40 、SiO 240 @CNTs 40 、SiO 280 @CNTs 40 、SiO 2120 @CNTs 40 、SiO 2160 @CNTs 40 . When other conditions remain unchanged, 35-EP / DTMS@PDA@SiO 2x @CNTs y Composite coating, explore the effect of CNTs and TEOS addition on the hydrophobic properties and surface morphology of the coating.
[0168] Fig.21Contact angle and sliding angle of the composite coating prepared with different CNTs and TEOS addition amounts. It can be seen from the figure that when only CNTs (0 / 40) is added to the coating without TEOS, the static contact angle of the coating is 114°, and the rolling angle is slightly greater than 30°; when 40mgTEOS and 40mgCNTs (1:1) are added to the coating, the static contact angle of the coating increases to 122°, and the rolling angle is slightly higher than 25°; when 80mgTEOS and 40mgCNTs are added to the coating, the static contact angle of the coating increases to 143°, and the rolling angle decreases to below 20°, and the hydrophobic performance is improved; when 120mgTEOS and 40mgCNTs are added to the coating, the static contact angle of the coating increases to 157°, and the rolling angle decreases to below 10°, and a superhydrophobic surface is successfully constructed; but when 160mgTEOS and 40mgCNTs are added to the coating, the superhydrophobic performance of the coating decreases, the static contact angle becomes 151°, and the rolling angle increases to more than 10°.
[0169] Example 12
[0170] In order to analyze the effect of different contents of DTMS@PDA@SiO2@CNTs nanoparticles on the surface of the composite coating, the proportions of DTMS@PDA@SiO2@CNTs in the coating were 0, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, and 35wt%, respectively, and the prepared EP / DTMS@PDA@SiO2@CNTs coatings were recorded as EP, 15-EP, 20-EP, 25-EP, 30-EP, and 35-EP. The surface roughness (Ra) of the composite coating was tested using a 3D confocal microscope, and the results are shown in Figure 2. Fig. 22 The roughness of pure epoxy coating is only 0.253μm. With the addition of DTMS@PDA@SiO2@CNTs, the microstructure of the composite coating surface is improved. When the addition amount of polymer particles is 30wt%, the roughness of the composite coating is 14.076μm, reaching the maximum roughness. When the addition amount of polymer particles is 35wt%, the roughness of the composite coating decreases.
[0171] Embodiment 13
[0172] The preparation method of EP / DTMS@PDA@SiO2@CNTs composite coating is the same as that of Example 11. The static contact angle (WCA) and sliding angle (SA) are shown in Fig.23. The static contact angle of the pure epoxy coating is only 80.26°, and the rolling angle is about 40°, that is, the pure epoxy surface is hydrophilic. This is because the surface of the pure epoxy resin coating is relatively smooth and the surface energy of the coating surface is relatively high. By adding DTMS@PDA@SiO2@CNTs particles, the roughness of the composite coating can be increased while the surface energy of the coating can be reduced. With the increase of the content of hydrophobic particles DTMS@PDA@SiO2@CNTs, the static contact angle of the EP / DTMS@PDA@SiO2@CNTs composite coating increases, and the rolling angle shows a downward trend. The addition of polymer particles significantly improves the hydrophobic properties of the coating. When the content of DTMS@PDA@SiO2@CNTs particles in the coating is 15wt%, the contact angle of the coating is 137.75°, and the rolling angle is reduced to about 15°; when the content of polymer particles in the coating is 20wt%, the contact angle of the coating is 143.09°, and the rolling angle is reduced to about 10°; when the content of polymer particles in the coating is 20wt%, the contact angle of the coating is 159.76°, at this time water droplets will bounce off quickly on the surface of the coating, that is, the rolling angle is reduced to 0, and the coating has superhydrophobic properties; when the content of polymer particles in the coating is 30wt%, the contact angle of the coating is 167.59°, and the rolling angle is 0, and the superhydrophobic property is further enhanced at this time; when the content of polymer particles in the coating is 35wt%, the contact angle of the coating is reduced to 141.86°, and the rolling angle is increased to about 10°. Through comparative analysis, it was found that when the proportion of DTMS@PDA@SiO2@CNTs particles in the composite coating was 30wt%, the superhydrophobic property of the composite coating was optimal.
[0173] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a DTMS@PDA@SiO2@CNTs composite material, comprising the following steps: dispersing graphitized carboxylated multi-walled carbon nanotubes in water-a first polar organic solvent to obtain a CNTs dispersion; Under alkaline conditions, the CNTs dispersion is mixed with tetraethyl silicate to perform an in-situ growth reaction, and nano-SiO2 is in-situ formed on the surface of the graphitized carboxylated multi-walled carbon nanotubes to obtain SiO2@CNTs; Providing a weak alkaline solvent; the pH value of the weak alkaline solvent is 7.5 to 9.5, and the weak alkaline solvent includes water and a second polar organic solvent; The SiO2@CNTs, the weak alkaline solvent, dopamine and dodecyltrimethylsilane DTMS are mixed to undergo an oxidative self-polymerization-hydrolysis reaction, wherein the dopamine self-polymerizes on the surface of the SiO2@CNTs to form polydopamine PDA, and simultaneously the DTMS is hydrolyzed to generate silanols that are grafted onto the surface of the SiO2@CNTs to obtain a DTMS@PDA@SiO2@CNTs composite material.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the tetraethyl silicate to the mass ratio of the graphitized carboxylated multi-walled carbon nanotubes in the CNTs dispersion is 3-4:
1.
3. The preparation method according to claim 1 or 2, characterized in that: The pH value of the alkaline condition is 8 to 10; the time of the in-situ growth reaction is 8 to 24 hours.
4. The preparation method according to claim 1, characterized in that: The mass ratio of dopamine to graphitized carboxylated multi-walled carbon nanotubes is 0.5-2:1; the mass ratio of DTMS to dopamine is 1-3:10; the temperature of the oxidative self-polymerization-hydrolysis reaction is 20-50°C, and the time is 12-24h.
5. The DTMS@PDA@SiO2@CNTs composite material prepared by the preparation method according to any one of claims 1 to 4 comprises SiO2@CNTs, PDA located on the surface of the SiO2@CNTs, and silanol chains grafted on the SiO2@CNTs; the silanol chains are obtained by hydrolysis of DTMS; the SiO2@CNTs comprise graphitized carboxylated multi-walled carbon nanotubes and nano-SiO2 grown in situ on the surface of the graphitized carboxylated multi-walled carbon nanotubes.
6. Use of the DTMS@PDA@SiO2@CNTs composite material according to claim 5 in a super-hydrophobic coating.
7. A super hydrophobic self-repairing anti-corrosion coating, characterized in that: The invention comprises epoxy resin, the DTMS@PDA@SiO2@CNTs composite material according to claim 5, a curing agent and an organic solvent.
8. The super hydrophobic self-repairing anti-corrosion coating according to claim 7, characterized in that: The mass of the DTMS@PDA@SiO2@CNTs composite material is 15-35% of the total mass of the epoxy resin, the curing agent and the DTMS@PDA@SiO2@CNTs composite material.
9. A super hydrophobic self-repairing anti-corrosion coating, characterized in that: The invention relates to a composite material comprising epoxy resin and the DTMS@PDA@SiO2@CNTs composite material according to claim 5 embedded in the epoxy resin.
10. The method for preparing the super hydrophobic self-repairing anti-corrosion coating according to claim 9, characterized in that: The method comprises the following steps: applying the super-hydrophobic self-repairing anti-corrosion coating according to claim 7 or 8 to the surface of a metal substrate, and curing the coating to obtain the super-hydrophobic self-repairing anti-corrosion coating.
Citation Information
Patent Citations
Super-hydrophobic cotton material with photothermal effect as well as preparation method and application of super-hydrophobic cotton material
CN113070043A
Super-hydrophilic carbon nanotube composite membrane and preparation method thereof
CN113893705A
Super-amphiphobic and super-weather-resistant organic silicon protective coating and preparation method thereof
CN115181495A
Super-hydrophobic marine antifouling coating and preparation method thereof
CN116554743A
Super-hydrophobic coating with self-repairing function and preparation method
CN116854380A