Carbon material surface TaC coating and preparation method thereof
The TaC coating prepared by slurry sintering method in a semiconductor crystal growth environment uses the combined structure of the transition layer and the surface layer to solve the problem of carbon material susceptible to silicon vapor erosion and high-temperature reactions, and improves service life and application Range, enhances anti-peel and density, and reduces cracking risk.
Patent Information
- Application Number
- CN202411076053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The surface of carbon materials in the semiconductor crystal environment is susceptible to silicon vapor erosion, resulting in surface damage and decreased strength. The existing TaC coating is prone to react with the environmental atmosphere at high temperatures, affecting product quality.
The TaC coating is prepared by slurry sintering method. Through the combined structure of the transition layer and the surface layer, the dense protective coating is formed by using components such as graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent. , solve the problem of thermal expansion difference and binding force between the coating and carbon matrix.
It significantly improves the service life and application range of carbon materials in semiconductor crystal growth environments, enhances the anti-peel characteristics and density of the coating, reduces the cracking risk of TaC coating, and improves corrosion and thermal shock resistance.
Smart Images

Figure BDA0004983413690000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor crystal growth, and in particular to a TaC coating on the surface of a carbon material and a preparation method thereof. Background Art
[0002] Semiconductor crystal growth is generally carried out in a high-temperature, high-purity environment, and the structural parts used are mainly made of carbon materials, such as carbon-carbon composite materials, graphite materials, etc. Since there are certain pores on the surface of commonly used carbon material structural parts and their corrosion resistance is low, they are easily corroded by silicon vapor when they are in a high-temperature semiconductor crystal growth environment for a long time, resulting in damage to the surface of the carbon material, pollution to the silicon crystal, and extreme decrease in the strength of the carbon material, which seriously affects the service life. The industry has made certain progress in SiC coating, but it is easy to react with the ambient atmosphere when doing semiconductor SiC epitaxy, affecting product quality. Because TaC has more excellent physical and chemical properties, its high-temperature chemical stability and corrosion resistance are much higher than SiC, and it can meet the high temperature of 2600℃. The use of TaC coating equipment can solve the problem of edge defects of semiconductor crystals and improve the quality of semiconductor crystals.
[0003] At present, the preparation methods of TaC coating mainly include molten salt method, sol-gel method, slurry sintering method, plasma spraying method, chemical vapor deposition (CVD), chemical vapor infiltration (CVI) and physical vapor deposition (PVD), etc. The present invention is based on the "slurry sintering method", adopts a special slurry formula and coating technique, and aims to provide a high-yield, low-cost TaC coating process, and improve the service life and application range of coated carbon parts in semiconductor crystal growth environments. Summary of the invention
[0004] In view of the above shortcomings of the prior art, the present invention provides a TaC coating for surface densification protection of carbon materials and a preparation method thereof, which is mainly used to improve the service life of carbon materials in the semiconductor field and expand the application scope of carbon materials in the semiconductor field. The preparation method provided by the present invention is mainly used to solve the coating cracking problem caused by the thermal expansion difference between the TaC coating and the carbon substrate, and improve the bonding force between the TaC coating and the carbon substrate.
[0005] Technical Solution
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] The present invention provides a TaC coating on the surface of a carbon material, comprising a transition layer and a surface layer.
[0008] The transition layer comprises graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent, and the graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent are mixed to obtain transition layer slurry, and the transition layer slurry is applied to the surface of the carbon material to form the transition layer;
[0009] The surface layer comprises TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent. The surface layer slurry is obtained by mixing TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent, and the surface layer slurry is applied to the side of the transition layer away from the carbon material to form the surface layer.
[0010] Furthermore, in parts by weight, the transition layer comprises:
[0011] 2-5 parts of graphite powder, 5-10 parts of phenolic resin, 1-2 parts of epoxy resin, 5-8 parts of anhydrous ethanol, 21-32 parts of distilled water and 0.002-0.005 parts of silane coupling agent.
[0012] Specifically, the preparation steps of the transition layer slurry are as follows:
[0013] 1) When preparing the transition layer slurry, firstly dissolve the phenolic resin PF7203 with the anhydrous ethanol, and fully stir to obtain a uniformly dissolved phenolic resin concentrated solution;
[0014] 2) slowly adding the distilled water into the concentrated phenolic resin solution, continuing to stir, fully dissolving and uniformly dissolving, to obtain a dilute phenolic resin solution;
[0015] 3) adding the epoxy resin AG-80 into the phenolic resin dilute solution, stirring and dissolving uniformly to obtain a resin mixed solution;
[0016] 4) adding the γ-aminopropyltriethoxysilane into the resin mixed solution and stirring evenly;
[0017] 5) Finally, the 800-mesh graphite powder is added to the above solution and stirred evenly to obtain the transition layer slurry.
[0018] Further, in parts by weight, the surface layer comprises:
[0019] 1-5 parts of TaC powder, 0.001-0.003 parts of boron oxide powder, 14-18 parts of phenolic resin, 10-15 parts of anhydrous ethanol, 33-45 parts of distilled water and 0.001-0.005 parts of silane coupling agent.
[0020] Specifically, the surface layer slurry preparation steps are as follows:
[0021] 1) When preparing the surface layer slurry, firstly dissolve the phenolic resin PF6908 with the anhydrous ethanol, and fully stir to obtain a uniformly dissolved phenolic resin concentrated solution;
[0022] 2) slowly adding the distilled water into the concentrated phenolic resin solution, continuing to stir, fully dissolving and uniformly dissolving, to obtain a phenolic resin solution;
[0023] 3) adding the γ-aminopropyltriethoxysilane into the phenolic resin solution and stirring evenly;
[0024] 4) Finally, the TaC powder and the boron oxide powder are mixed evenly, added into the above solution, and stirred sufficiently to obtain the surface layer slurry.
[0025] The graphite powder is mainly used to fill the pores on the surface of the carbon matrix and provide a larger contact surface for the surface layer slurry coating. The phenolic resin plays the role of a curing agent for the epoxy resin while playing an adhesive role. The epoxy resin can greatly improve the adhesion between the slurry and the carbon matrix. The silane coupling agent mainly plays the role of increasing the affinity between the phenolic resin, epoxy resin and graphite powder, carbon matrix, TaC, and boron oxide. Through physical entanglement and chemical reaction, a stronger chemical bond is formed to improve the compactness between the resin and the carbon material, TaC, and boron oxide. The TaC powder and boron oxide powder react and combine with other substances under high temperature conditions to improve the density of the carbon matrix surface coating and the toughness of the coating. The anhydrous ethanol and distilled water are mixed to form the main solvent of the slurry component, reduce the viscosity of the resin, and increase the dispersion of other components to improve the uniformity of the coating. The phenolic resin and epoxy resin, while playing an adhesive role, provide expansion space for other substances after carbonization, and provide a transition zone for the difference in thermal expansion of different components.
[0026] Furthermore, the graphite powder is 800-1000 mesh high-purity flake graphite powder with a carbon content of ≥99.99%;
[0027] Preferably, the graphite powder is 1000 mesh high-purity flake graphite powder with a carbon content of ≥99.99%;
[0028] Optionally, the slurry uses a phenolic resin that is a resol-soluble thermosetting phenolic resin liquid with a residual carbon content of 40%-45%;
[0029] Optionally, the slurry uses phenolic resin from Jinan Shengquan Group Co., Ltd., and the selected models are PF7203 and PF6908, the PF7203 is used for the transition layer slurry, and the PF6908 is used for the surface layer slurry;
[0030] Optionally, the epoxy resin selected for the slurry is a glycidylamine type epoxy resin liquid, and the selected model is AG-80 or AFG-90;
[0031] Optionally, the slurry is made of epoxy resin from a common commercial source, and the selected brand is AG80;
[0032] Optionally, the silane coupling agent selected for the slurry is γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethylaminosilane or benzylaminomethyltriethoxysilane.
[0033] Optionally, the silane coupling agent selected for the slurry is γ-aminopropyltriethoxysilane or N-phenylaminomethyltriethoxysilane.
[0034] Optionally, the slurry uses TaC powder with a particle size of 0.5-1.5 μm and a purity greater than 99.99%;
[0035] Optionally, the boron oxide powder selected for the slurry is ultrafine high-purity boron oxide powder with a particle size of 2500 mesh and a purity greater than 99.9%.
[0036] Further, the thickness of the TaC coating is 30-150 microns;
[0037] Wherein, the thickness of the transition layer is 30-50% of the total thickness of the coating; the thickness of the surface layer is 50-70% of the total thickness of the coating.
[0038] A method for preparing a TaC coating on a carbon material surface comprises the following steps:
[0039] (1) Pretreatment of carbon substrate;
[0040] (2) Preparation and coating of transition layer slurry: preparing transition layer slurry with graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent in a certain weight ratio; after the transition layer slurry is evenly sprayed on the surface of the high-purity carbon substrate, the transition layer slurry is placed in an oven at a constant temperature of 180-200° C. for 3-5 hours to achieve the curing of the transition layer slurry;
[0041] (3) Preparation and coating of surface layer slurry: preparing surface layer slurry with TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent in a certain weight ratio; after the surface layer slurry is evenly sprayed on the surface of the cured transition layer, the surface layer slurry is placed in an oven at a constant temperature of 180-200° C. for 3-5 hours to achieve curing of the surface layer slurry;
[0042] (4) A carbon material containing a TaC coating is obtained through a deposition and sintering process.
[0043] Furthermore, in the step (4), during the deposition process, nitrogen and propane are mixed at a flow rate ratio of 5-20:1 at a deposition temperature of 1050-1200°C and a vacuum degree of 900-1000 Pa, and then the mixture is heated at a rate of 0.2-0.5 m / s. 3 The deposition rate was 20-30 h at a rate of / min.
[0044] Furthermore, in the step (4), during the sintering process, under the conditions of a temperature of 2000-2500°C and a vacuum degree of 50-80Pa, after maintaining the constant temperature for 30-60 minutes, argon is introduced at a rate of 0.3-0.4m3 / min, the vacuum degree after the introduction of argon is 1500-2000Pa, and sintering is continued for 4-5 hours.
[0045] Specifically, in step (4), the sample after the surface layer slurry is cured is placed in a CVD furnace, and nitrogen and alkane propylene gas are mixed in a mass ratio of 10-20:1 at a temperature of 1200°C and a vacuum degree of 500-800Pa, and then 0.2-0.5m 3 After the CVD deposition is completed, the sample is placed in a sintering furnace. After 30-60 minutes of constant temperature at a temperature of 2000-2500°C and a vacuum degree of 50-80Pa, the sample is deposited at a rate of 0.3-0.4m / min. 3 Argon is introduced at a rate of 1500-2000 Pa after the introduction of argon, and sintering is continued for 4-5 hours. After sintering, a dense and uniform TaC coating carbon component with a coating thickness of 30-120 microns is obtained.
[0046] Furthermore, in the step (1), the carbon substrate is pretreated by placing the carbon substrate in an ultrasonic bath, cleaning the surface stains and dust, and then drying the carbon substrate, and performing high-temperature purification at 2500° C. in a purification furnace to obtain a high-purity carbon substrate.
[0047] Beneficial Effects
[0048] Compared with the known public technology, the technical solution provided by the present invention has the following beneficial effects:
[0049] 1. Through ultrasonic cleaning and high-temperature purification of the carbon matrix, the dust stains attached to the surface and other impurities of the product are removed to obtain a high-purity carbon matrix with a clean surface. In the special environment of semiconductor crystal growth, the product will not produce other special impurity gases, completely eliminating the risk of coating blistering. At the same time, it also improves the wettability of the coating and the product surface, greatly enhancing the anti-peeling properties of the coating.
[0050] 2. By spraying and curing the transition layer slurry, an appropriate amount of graphite powder, phenolic resin, epoxy resin and other substances are introduced to the surface of the carbon matrix. With the back-end curing, CVD deposition, sintering and other processes, the cross-linking strength between the transition layer components and the surface of the carbon matrix is improved, while the density of the surface of the carbon matrix is improved. In addition, as the phenolic resin and epoxy resin are converted into resin carbon with a thermal expansion coefficient different from that of the carbon matrix-based graphite powder, together with the graphite powder, a transition layer coating with a thermal expansion coefficient higher than that of the carbon matrix but lower than that of the TaC coating is formed, providing a buffer zone for the difference in thermal expansion coefficients between the TaC coating and the carbon matrix, reducing the risk of cracking of the TaC coating.
[0051] 3. The introduction of boron oxide into the surface layer slurry effectively improves the sintering degree of the TaC coating, catalytically promotes the uniformity of the coating thickness, and the bonding strength between the TaC coating and the transition layer and the carbon matrix, thereby improving the surface density of the product.
[0052] 4. Phenolic resin, epoxy resin and silane coupling agent are introduced into the slurry at the same time, which improves the cross-linking strength between the slurry and the substrate during the spraying stage and ensures the uniformity of the coating thickness; during the CVD deposition and sintering stages, while ensuring the connection strength of each component, the resin undergoes a series of structural transformations such as carbonization and graphitization, providing space for the filling of pyrolytic carbon produced by CVD deposition and the thermal expansion of other components, so as to solve the problem of mismatched thermal expansion of each component.
[0053] 5. The TaC coated carbon parts prepared by the present invention have better corrosion resistance and thermal shock resistance and longer service life. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The present invention will be further described below in conjunction with the embodiments.
[0056] The manufacturers and models of the raw materials used in the embodiments and comparative examples are as follows:
[0057] Carbon-carbon composite material sample, VU-CC from Hangzhou Weiken New Material Technology Co., Ltd., density 1.50g / cm 3 ;
[0058] Graphite powder (800 mesh), Shenzhen Hanhui Graphite Co., Ltd.;
[0059] Graphite powder (1000 mesh), Shenzhen Hanhui Graphite Co., Ltd.;
[0060] Phenolic resin PF7203, Jinan Shengquan Group Co., Ltd.;
[0061] Phenolic resin PF6908, Jinan Shengquan Group Co., Ltd.;
[0062] Epoxy resin AG-80, Yixin Chemical New Materials;
[0063] γ-Aminopropyltriethoxysilane, KH550, Jinan Yunuo Chemical Co., Ltd.;
[0064] TaC powder, TaC-3 from Hunan Huasisheng Technology Co., Ltd.;
[0065] Boron oxide powder, Jinan Yunuo Chemical Co., Ltd. YN;
[0066] N-phenylaminomethyltriethoxysilane, KH-ND42, Hangzhou Jessica Chemical Co., Ltd.;
[0067] Isostatic graphite sample, Hangzhou VU-G-OF New Material Technology Co., Ltd.
[0068] (I) Embodiment
[0069] Example 1
[0070] A TaC coating on the surface of a carbon material and a preparation method thereof, comprising the following steps:
[0071] S1, density 1.30g / cm 3 The carbon-carbon composite material sample is placed in an ultrasonic bath pot, and distilled water is added to completely immerse it and then washed for 10-30 minutes to obtain a surface-cleaned water-containing carbon-carbon sample. The water-containing carbon-carbon sample is placed in a dust-free oven, and the temperature is increased from room temperature to 150°C at a rate of 2°C / min, and the temperature is kept at 150°C for 3-4 hours to obtain a dry clean carbon-carbon sample. The clean carbon-carbon sample is purified at high temperature at 2500°C in a purification furnace to obtain a high-purity carbon-carbon sample.
[0072] S2. A transition layer slurry is prepared from 800 mesh graphite powder, phenolic resin PF7203, epoxy resin AG-80, anhydrous ethanol, distilled water and γ-aminopropyl triethoxysilane in a weight ratio of 3:5:1:6:22:0.002. The method comprises the following steps:
[0073] 1) When preparing the transition layer slurry, firstly dissolve the phenolic resin PF7203 with the anhydrous ethanol, and fully stir to obtain a uniformly dissolved phenolic resin concentrated solution.
[0074] 2) slowly adding the distilled water into the concentrated phenolic resin solution, continuing to stir, fully dissolving and uniformly dissolving, to obtain a dilute phenolic resin solution with a mass concentration of about 16.13%.
[0075] 3) adding the epoxy resin AG-80 into the phenolic resin dilute solution, stirring and dissolving the mixture uniformly to obtain a resin mixed solution.
[0076] 4) adding the γ-aminopropyltriethoxysilane into the resin mixed solution and stirring evenly.
[0077] 5) Finally, the 800-mesh graphite powder is added to the above solution and stirred evenly to obtain the transition layer slurry.
[0078] S3. After the transition layer slurry is evenly sprayed on the surface of the high-purity carbon substrate, it is inverted every 10 minutes and air-dried for 1 hour, then placed in an oven and heated to 80°C at a heating rate of 5°C / min and kept at a constant temperature for 15 minutes, and then heated to 180°C at a heating rate of 2°C / min and kept at a constant temperature for 180 minutes. The transition layer slurry is cured to obtain a transition layer coating part.
[0079] S4. A surface layer slurry is prepared from TaC powder, boron oxide powder, phenolic resin PF6908, anhydrous ethanol, distilled water, γ-aminopropyltriethoxysilane and other substances in a weight ratio of 5:0.002:15:15:40:0.001. The method comprises the following steps:
[0080] 1) When preparing the surface layer slurry, firstly dissolve the phenolic resin PF6908 in the anhydrous ethanol, and stir thoroughly to obtain a uniformly dissolved phenolic resin concentrated solution.
[0081] 2) slowly adding the distilled water into the concentrated phenolic resin solution, continuing to stir, fully dissolving and uniformly dissolving, to obtain a phenolic resin solution with a mass concentration of about 21.43%.
[0082] 3) adding the γ-aminopropyltriethoxysilane into the phenolic resin solution and stirring the mixture evenly.
[0083] 4) Finally, the TaC powder and the boron oxide powder are mixed evenly, added into the above solution, and stirred sufficiently to obtain the surface layer slurry.
[0084] S5, after the surface layer slurry is evenly sprayed on the surface of the transition layer coating part, the surface layer slurry is solidified to obtain a preliminary coating part in the same manner as step S3.
[0085] S6. Place the above-mentioned preliminary coated parts into a CVD furnace and operate according to the following process:
[0086] 1) The first step: evacuate the furnace to a pressure of 0.3 KPa;
[0087] 2) Step 2: Fill with nitrogen until the furnace pressure is 80±10KPa;
[0088] 3) Step 3: Adjust the nitrogen flow rate and vacuum pump opening to keep the furnace pressure at 80±10KPa;
[0089] 4) Step 4: Raise the temperature from room temperature to 500°C for 120 minutes, with a furnace pressure of 80±10KPa;
[0090] 5) Step 5: 500°C, constant temperature for 30 minutes, furnace pressure 80±10KPa;
[0091] 6) Step 6: Heat from 500°C to 800°C for 90 minutes, furnace pressure 80±10KPa;
[0092] 7) Step 7: 800°C, constant temperature for 30 min, furnace pressure 80±10KPa;
[0093] 8) Step 8: Heating from 800°C to 1000°C for 90 minutes, furnace pressure 80±10KPa;
[0094] 9) Step 9: 1000°C, constant temperature for 120 min, furnace pressure 80±10KPa;
[0095] 10) Step 10: Turn off the nitrogen, continue to evacuate until the furnace pressure remains at 0.3-0.5KPa, and heat from 1000℃ to 1050℃ for 30 minutes;
[0096] 11) Step 11: After nitrogen flow and propane flow are mixed at a ratio of 10:1, they are introduced into the CVD furnace, the vacuum pump is continuously operated, the furnace pressure is 0.9-1.0 KPa, and the temperature is kept at 1050±10℃ for 1500min;
[0097] 12) Step 12: Turn off propane, continue to pass nitrogen, keep the vacuum pump running, furnace pressure 0.5-0.6KPa, constant temperature 1050±10℃ for 60min;
[0098] 13) Step 13: Turn off the heating, continue to pass nitrogen, keep the vacuum pump running, the furnace pressure is 0.5-0.6KPa, and start cooling;
[0099] 14) Step 14: Cool down to 500°C, increase nitrogen flow, keep the vacuum pump running, keep the furnace pressure at 80-90KPa, and keep cooling;
[0100] 15) Step 15: Cool down to below 100°C, turn off the vacuum pump, fill with nitrogen to adjust the furnace pressure to normal pressure, then turn off the nitrogen, open the furnace cover, complete the initial carbonization of the coating parts, and obtain the coated carbonized parts.
[0101] S7. Place the coated carbonized parts into a sintering furnace and operate according to the following process:
[0102] 1) The first step: vacuum to 50-80Pa;
[0103] 2) Step 2: Raise the temperature from room temperature to 500°C for 90 minutes, with a furnace pressure of 50-80Pa;
[0104] 3) Step 3: 500°C, constant temperature for 10 minutes, furnace pressure 50-80Pa;
[0105] 4) Step 4: Heat from 500°C to 1000°C for 100 minutes, furnace pressure 50-80Pa;
[0106] 5) Step 5: 1000℃, constant temperature for 30min, furnace pressure 50-80Pa;
[0107] 6) Step 6: Heating from 1000°C to 1500°C for 120 minutes, furnace pressure 50-80Pa;
[0108] 7) Step 7: 1500°C, constant temperature for 30 minutes, furnace pressure 50-80Pa;
[0109] 8) Step 8: Heating from 1500°C to 2000°C for 150 minutes, furnace pressure 50-80Pa;
[0110] 9) Step 9: 2000°C, constant temperature for 60 minutes, furnace pressure 50-80Pa;
[0111] 10) Step 10: Heating from 2000°C to 2400°C for 180 minutes, furnace pressure 50-80Pa;
[0112] 11) Step 11: 2400°C, constant temperature for 60 minutes, furnace pressure 50-80Pa;
[0113] 12) Step 12: 2400℃, 0.35m argon 33 / min, furnace pressure 1700±200Pa, sintering 300min;
[0114] 13) Step 13: Turn off the argon gas, evacuate to 50-80Pa, turn off the heating, and start cooling;
[0115] 14) Step 14: Cool down to below 50°C, turn off the vacuum pump, pass nitrogen to normal pressure and then turn off the nitrogen, open the furnace cover and take out the sample.
[0116] The sintering of the coated carbide part is completed through the above steps to obtain a carbon-carbon sample with a uniform and dense TaC coating, wherein the thickness of the TaC coating is 120 microns, the thickness of the transition layer is 50 microns, and the thickness of the surface layer is 70 microns.
[0117] Example 2
[0118] The method in Example 1 was followed, except that the transition layer slurry components were replaced with 1000 mesh graphite powder, phenolic resin PF7203, epoxy resin AG-80, anhydrous ethanol, distilled water and γ-aminopropyltriethoxysilane in a weight ratio of 5:5:1:5:25:0.003.
[0119] Example 3
[0120] The method in Example 1 was followed, except that the γ-aminopropyltriethoxysilane in the transition layer slurry and the surface layer slurry was replaced with N-phenylaminomethyltriethoxysilane in equal amounts.
[0121] Example 4
[0122] The method in Example 1 is followed, except that the carbon-carbon composite material sample is changed to an isostatically pressed graphite sample.
[0123] The method in Example 1 was followed, except that the transition layer slurry components were replaced with 1000 mesh graphite powder, phenolic resin PF7203, epoxy resin AG-80, anhydrous ethanol, distilled water and γ-aminopropyltriethoxysilane in a weight ratio of 2:8:2:8:24:0.005.
[0124] The method in Example 1 was followed, except that the surface layer slurry components were replaced with TaC powder, boron oxide powder, phenolic resin PF6908, anhydrous ethanol, distilled water and γ-aminopropyltriethoxysilane in a weight ratio of 5:0.003:15:15:35:0.005.
[0125] Example 5
[0126] The method in Example 4 was followed, except that the γ-aminopropyltriethoxysilane in the transition layer slurry and the surface layer slurry was replaced with N-phenylaminomethyltriethoxysilane in equal amounts.
[0127] Comparative Example 1
[0128] The method in Example 1 is followed, except that the carbon-to-carbon sample is not subjected to ultrasonic cleaning and high-temperature purification treatment.
[0129] Specifically: step S1 is missing.
[0130] Comparative Example 2
[0131] The method in Example 1 is followed, except that the transition layer slurry is not sprayed and cured.
[0132] Specifically: Step S2 and Step S3 are missing.
[0133] Comparative Example 3
[0134] The method in Example 1 is followed, except that the phenolic resin PF7203, the epoxy resin AG-80 and the γ-aminopropyltriethoxysilane are not added to the transition layer slurry;
[0135] Specifically, the transition layer slurry is made of 800 mesh graphite powder, anhydrous ethanol and distilled water in a weight ratio of 3:6:22.
[0136] Comparative Example 4
[0137] The method in Example 4 is followed, except that the isostatically pressed graphite sample is not subjected to ultrasonic cleaning and high-temperature purification treatment.
[0138] Specifically: step S1 is missing.
[0139] Comparative Example 5
[0140] The method in Example 4 is followed, except that the transition layer slurry is not sprayed and cured.
[0141] Specifically: Step S2 and Step S3 are missing.
[0142] Comparative Example 6
[0143] The method in Example 4 is followed, except that no phenolic resin PF7203, epoxy resin AG-80 and γ-aminopropyltriethoxysilane are added to the transition layer slurry.
[0144] Specifically, the transition layer slurry components are 1000 mesh graphite powder, anhydrous ethanol, and distilled water in a weight ratio of 2:8:24.
[0145] Comparative Example 7
[0146] The method of Example 1 was followed, except that no boron oxide powder was added to the surface layer slurry.
[0147] Comparative Example 8
[0148] The method of Example 4 was followed, except that no boron oxide powder was added to the surface layer slurry.
[0149] (II) Performance test
[0150] In order to consider the coating effect of the samples of Examples 1-5 and Comparative Examples 1-8, as well as the corrosion resistance in silicon vapor, the above-prepared samples were subjected to relevant tests. The main test items and methods are as follows:
[0151] (1) Coating status: Visually inspect the coating surface for bulges and cracks;
[0152] (2) Porosity: Tested in accordance with GB / T24529-2009 Method for Determination of Apparent Porosity of Carbon Materials;
[0153] (3) Corrosion resistance: First, place the silicon material in a graphite crucible, place each sample on the graphite crucible, cover the graphite crucible, make the silicon vapor contact the sample on one side, then place the crucible in the test furnace, heat it to 1600℃ at a rate of 5℃ / min and keep it warm for 100h. High-purity argon is used for protection throughout the experiment. After cooling down and taking out of the furnace, the bending strength test of the sample is carried out in accordance with "GB / T40398.2-2021 Test Method for Carbon-Carbon Composite Carbon Materials Part 2: Bending Performance Test". After the silicon material is melted, a large amount of silicon vapor will be generated, which diffuses to the surface of the carbon material to undergo a silicification reaction, thereby reducing the mechanical properties of the sample.
[0154] The test results are shown in Table 1 below:
[0155] Table 1
[0156]
[0157] With reference to Example 1 and Example 2, it can be seen that the product made of 1000 mesh graphite powder as a transition layer component has lower porosity, stronger bending strength, better corrosion resistance and longer service life than that made of 800 mesh graphite powder. With reference to Example 1 and Example 3, and with reference to Example 4 and Example 5, it can be seen that γ-aminopropyltriethoxysilane and N-phenylaminomethyltriethoxysilane have no obvious influence on the difference in material.
[0158] Referring to Example 1 and Comparative Example 1, and referring to Example 4 and Comparative Example 4, it can be seen that the cleanliness of the substrate has a significant effect on the stability of the coating. The higher the purity of the substrate, the better the coating wrapping state, the lower the porosity of the sample, and the stronger the corrosion resistance.
[0159] With reference to Example 1 and Comparative Example 2, and with reference to Example 4 and Comparative Example 5, it can be seen that the transition layer slurry provides a buffer zone for the difference in thermal expansion coefficient between the TaC coating and the carbon substrate, thereby reducing problems such as cracking and peeling of the TaC coating, significantly slowing down the rate of performance degradation, and improving corrosion resistance.
[0160] With reference to Example 1 and Comparative Example 3, and with reference to Example 4 and Comparative Example 6, it can be seen that the phenolic resin, epoxy resin, and silane coupling agent improve the crosslinking strength between the slurry and the substrate in the coating, and alleviate the peeling problem of the coating.
[0161] With reference to Example 1 and Comparative Example 7, and with reference to Example 4 and Comparative Example 8, it can be seen that the boron oxide powder plays the role of a sintering agent in the coating, reduces the surface porosity, and improves the corrosion resistance.
[0162] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present invention.
Claims
1. A TaC coating on the surface of a carbon material, characterized in that: Including transition layer and surface layer, The transition layer comprises graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent, and the graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent are mixed to obtain transition layer slurry, and the transition layer slurry is applied to the surface of the carbon material to form the transition layer; The surface layer comprises TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent. The surface layer slurry is obtained by mixing TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent, and the surface layer slurry is applied to the side of the transition layer away from the carbon material to form the surface layer.
2. The TaC coating on the surface of a carbon material according to claim 1, characterized in that: In parts by weight, the transition layer comprises: 2-5 parts of graphite powder, 5-10 parts of phenolic resin, 1-2 parts of epoxy resin, 5-8 parts of anhydrous ethanol, 21-32 parts of distilled water and 0.002-0.005 parts of silane coupling agent.
3. The TaC coating on the surface of a carbon material according to claim 2, characterized in that: By weight, the surface layer comprises: 1-5 parts of TaC powder, 0.001-0.003 parts of boron oxide powder, 14-18 parts of phenolic resin, 10-15 parts of anhydrous ethanol, 33-45 parts of distilled water and 0.001-0.005 parts of silane coupling agent.
4. The TaC coating on the surface of a carbon material according to claim 3, characterized in that: The graphite powder is 800-1000 mesh high-purity flake graphite powder with a carbon content of ≥99.99%; The silane coupling agent is γ-aminopropyltriethoxysilane or N-phenylaminomethyltriethoxysilane; The TaC powder has a particle size of 0.5-1.5 μm and a purity greater than 99.99%; The particle size of the boron oxide powder is 2500 meshes, and the purity is greater than 99.9%.
5. The TaC coating on the surface of a carbon material according to claim 1, characterized in that: The thickness of the TaC coating is 30-120 microns; Wherein, the thickness of the transition layer is 30-50% of the total thickness of the coating; the thickness of the surface layer is 70-50% of the total thickness of the coating.
6. A method for preparing a TaC coating on a carbon material surface as claimed in any one of claims 1 to 5, characterized in that: It includes the following steps: (1) Pretreatment of carbon substrate; (2) Preparation and coating of transition layer slurry: preparing transition layer slurry with graphite powder, phenolic resin, epoxy resin, anhydrous ethanol, distilled water and silane coupling agent in a certain weight ratio; spraying the transition layer slurry evenly on the surface of the high-purity carbon substrate and curing it at 180-200° C. to obtain; (3) Preparation and coating of surface layer slurry: preparing surface layer slurry with TaC powder, boron oxide powder, phenolic resin, anhydrous ethanol, distilled water and silane coupling agent in a certain weight ratio; spraying the surface layer slurry evenly on the surface of the cured transition layer, and curing at 180-200° C. to obtain; (4) A carbon material containing a TaC coating is obtained through a deposition and sintering process.
7. The method for preparing a TaC coating on a carbon material surface according to claim 6, characterized in that: In the step (4), during the deposition process, under the conditions of a deposition temperature of 1050-1200°C and a vacuum degree of 900-1000 Pa, nitrogen and propane gas are mixed at a flow ratio of 5-20:1 and then heated at 0.2-0.5 m 3 The deposition rate was 20-30 h at a rate of / min.
8. The method for preparing a TaC coating on a carbon material surface according to claim 6, characterized in that: In the step (4), during the sintering process, the temperature is 2000-2500°C and the vacuum degree is 50-80Pa. After the temperature is kept constant for 30-60 minutes, the sintering temperature is 0.3-0.4m 3 Argon is introduced at a rate of 1500-2000 Pa and sintering is continued for 4-5 h.
9. The method for preparing a TaC coating on a carbon material surface according to claim 6, characterized in that: In the step (1), the carbon substrate is pretreated by placing the carbon substrate in an ultrasonic bath, cleaning the surface stains and dust, and then drying the carbon substrate. The carbon substrate is purified at high temperature at 2500° C. in a purification furnace to obtain a high-purity carbon substrate.
10. The method for preparing a TaC coating on a carbon material surface according to claim 6, characterized in that: In the steps (2) and (3), the curing time is 3-5 hours.
Citation Information
Patent Citations
Preparation method of anti-oxidization carbon-carbon composite heat isolation material
CN106116626A
High-toughness ultrahigh-temperature ceramic-based composite material and preparation method thereof
CN114044679A
Ablation-resistant thermal shock-resistant zirconium silicate-high-alumina glass / HTBS high-entropy ceramic coating as well as preparation method and application thereof
CN114605173A
Method for growing TaC coating on surface of graphite-based material
CN114956825A
Method for preparing tantalum carbide coating by CVD (chemical vapor deposition) method
CN115948721A
Cited By
Multilayer antioxidant carbon aerogel composite material and preparation method and application thereof
CN122233819A
A multi-layer antioxidant carbon aerogel composite material and a preparation method and application thereof
CN122233819B