Method for preparing graphene oxide-based waterborne polyurethane marine anticorrosive coating
By modifying graphene oxide with phytic acid-doped melamine, a GO/PA-AT composite was prepared and mixed with waterborne polyurethane. This solved the problem of insufficient anti-corrosion performance of waterborne polyurethane coatings in marine environments and achieved a highly efficient corrosion protection effect.
Patent Information
- Application Number
- CN202411315390.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-22
AI Technical Summary
Existing waterborne polyurethane coatings have insufficient anti-corrosion performance in marine environments. The uneven dispersion and poor compatibility of nano-graphene in coatings limit the application of graphene in anti-corrosion coatings, and traditional methods are either costly or have short-lived effects.
A GO/PA-AT composite was prepared by non-covalent functionalization modification of graphene oxide using phytic acid-doped melamine, and then mixed with waterborne polyurethane to form a graphene oxide-based waterborne polyurethane marine anti-corrosion coating.
It improves the dispersion uniformity of graphene oxide in waterborne polyurethane and the mechanical properties of the coating, significantly enhances the corrosion protection efficiency of carbon steel in seawater environment, and the coating has high hardness, strong adhesion and excellent impact resistance.
Smart Images

Figure CN118995024A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to a method for preparing a graphene oxide-based waterborne polyurethane marine anticorrosive coating. Background Art
[0002] Metal corrosion is ubiquitous and is the most important cause of natural loss of many types of metal-related equipment. According to statistics, the economic losses caused by corrosion worldwide are about 800 billion to 100 billion US dollars each year, which is more than six times the combined losses caused by natural disasters such as earthquakes and floods. A large amount of steel is used in transportation, chemical industry, construction, infrastructure, railways and marine development, resulting in increasingly serious steel corrosion.
[0003] At present, the corrosion and protection of the marine environment mainly rely on the protection of the external coating, that is, the coating can give full play to the resistance effect, shielding effect, cathodic protection effect and passivation corrosion inhibition effect to achieve better anti-corrosion effect. Traditional oily organic coatings are poor in environmental protection and the physical and chemical properties of the film layer are insufficient. Waterborne Polyurethane (WPU) coatings with excellent flexibility, wear resistance, weather resistance, environmental protection and non-toxicity are selected, and water is used as a dispersion medium, which has also been widely used. However, pure waterborne polyurethane has poor water resistance and corrosion resistance due to the presence of hydrophilic groups on its main chain or side chain, so it is limited in practical applications. Modifying the polyurethane itself to improve its performance is difficult to meet the current increasingly stringent application requirements. In recent years, some studies have confirmed that the mechanical, thermodynamic, anti-corrosion, and water-resistant properties of waterborne polyurethane can be effectively improved by adding high specific surface area or small size nanoparticles. However, whether the nanomaterial can be evenly and well dispersed in the polymer matrix is the most important factor affecting the performance of nanomaterial-polymer composites.
[0004] Graphene with a six-membered ring honeycomb structure has excellent properties in mechanics, heat, electricity, optics, quantum mechanics, etc. At the same time, due to its high electrical conductivity, high thermal conductivity and excellent mechanical properties, it has attracted widespread attention in the fields of energy, sensors and semiconductors. At present, the method of selecting graphene and its derivatives as nanofillers has been documented, but the graphene or graphene oxide in the filler is easy to agglomerate due to its high specific surface area and strong van der Waals force between adjacent layers, and the compatibility of graphene with the coating base resin is very poor, which limits the application of graphene in the coating industry.
[0005] In further research on corrosion protection coatings, graphene can not only protect the substrate material from the effects of violent chemical reactions, but also its antioxidant ability and oxygen barrier properties have gradually attracted attention. However, as far as the current status of marine corrosion protection in my country is concerned, innovative research on graphene has emerged in an endless stream, but none of them has been further verified and applied, and the mechanism research has not been in-depth. The cost of directly depositing a graphene corrosion-resistant layer on the metal surface by CVD is high, and the equipment requirements are high; the transfer process of the graphene assembly transfer method requires corrosion of the substrate material, which will affect the quality of the graphene layer itself; the graphene spraying method has not yet found the best process to obtain a large area of continuous and uniform film layer; the composite coating still needs further research, and these methods cannot meet the requirements of industrialization for the time being. At the same time, some studies have found that graphene only has an effective anti-corrosion effect in the short term. For example, graphene has obvious anti-thermal oxidation and anti-electrochemical oxidation effects on the substrate copper in the short term, but in long-term experiments, graphene has accelerated the oxidative corrosion of the substrate copper in the room temperature air environment. These issues are worthy of further research and discussion. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a method for preparing a graphene oxide-based waterborne polyurethane marine anticorrosion coating.
[0007] In order to achieve the above object, the present invention provides the following technical solutions: 1. A method for preparing a graphene oxide-based waterborne polyurethane marine anticorrosion coating, comprising the following preparation steps: (1) Preparation of phytic acid-doped triphenylamine The tripolyaniline and phytic acid are mixed, ultrasonicated at room temperature for 30 minutes, the resulting precipitate is collected by filtration, the solid product is washed with distilled water, and then dried to obtain the product; (2) Preparation of graphene oxide / phytic acid-doped triphenylamine Graphene oxide and phytic acid-doped triphenylamine were mixed and added into deionized water, and then ultrasonicated for 1 h to obtain a uniformly dispersed GO / PA-AT mixed solution; (3) Preparation of GO / PA-AT water-based composite coating The GO / PA-AT mixed liquid was mixed with the waterborne polyurethane curing agent and stirred at high speed for 10 minutes, then added into the waterborne polyurethane solution and emulsified into a uniform emulsion under high-speed stirring for 10 minutes to obtain a graphene oxide-based waterborne polyurethane marine anticorrosive coating material.
[0008] Preferably, the present invention further comprises the step of preparing tripolyaniline: dissolving p-phenylenediamine sulfate and aniline in an aqueous solution of HCl, adding ammonium persulfate, stirring at room temperature for 1 hour, collecting the resulting precipitate by filtration and washing it with an aqueous solution of HCl, washing the solid product with ammonia water and then rinsing it with a large amount of distilled water, and then drying it at 60°C.
[0009] Preferably, in step (1), the mass ratio of tripolyaniline to phytic acid when mixed is 1:1-5.
[0010] It is further preferred that in step (1), the mass ratio of trianiline to phytic acid when mixed is 1:2.
[0011] Preferably, in step (2), the mass ratio of graphene oxide to phytic acid-doped triphenylamine is 1:1-5.
[0012] The present invention is further preferred that in step (2), the mass ratio of graphene oxide to phytic acid-doped triphenylamine is 1:3.
[0013] Preferably, in step (3), the mass ratio of the GO / PA-AT mixed solution to the aqueous polyurethane is 0.4-1.2:95.
[0014] Preferably, in step (3), the mass ratio of GO / PA-AT to waterborne polyurethane is 0.4-1.2:95.
[0015] It is further preferred that in step (3), the mass ratio of GO / PA-AT to waterborne polyurethane is 0.8:95.
[0016] Preferably, in step (3), the amount of the waterborne polyurethane curing agent used is 3 wt % of the waterborne polyurethane.
[0017] The beneficial effects of the present invention are as follows: the present invention prepares a phytic acid-doped triphenylamine (PA-AT) to perform non-covalent functionalization modification on GO to obtain GO / PA-AT, and the composite reduces the self-agglomeration behavior of graphene oxide and improves its uniformity in the dispersion medium. It is added to waterborne polyurethane as a filler to synthesize a functionalized graphene oxide waterborne composite coating. The preparation method is simple, the process conditions are mild, and after the prepared coating is used on the surface of carbon steel material, the corrosion protection efficiency of carbon steel in seawater environment can be significantly improved, and the mechanical properties of the coating are excellent, such as high hardness, strong adhesion, and strong impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration: Figure 1 The preparation process of the composite coating.
[0019] Figure 2 Infrared spectra of AT (A) and PA-AT (B).
[0020] Figure 3 XPS spectra of GO and its composites; (A) XPS elemental spectrum of GO and GO / PA-AT, (B) C1s spectrum of GO, (C) C1s spectrum of GO / PA-AT and (D) N1s spectrum.
[0021] Figure 4 SEM images of GO (A), PA-AT (B) and GO / PA-AT (C).
[0022] Figure 5 Electrochemical performance test diagrams of different coating samples; (A) Nyquist diagram, (B) Bode impedance modulus diagram, (C) Bode phase angle diagram.
[0023] Figure 6 Tafel diagrams of different coating samples.
[0024] Figure 7 Impact resistance tests of WPU samples with different composite filler compositions at heights of 50 cm (A), 45 cm (B), 40 cm (C), GO / WPU 50 cm (D), GO / PA-AT / WPU 50 cm (E), and hardness test results of WPU, GO / WPU and WPU coatings with different mass ratios of graphene oxide to PA-AT (F).
[0025] Figure 8 The adhesion of WPU samples with different composite fillers before and after the salt spray test (A) and the adhesion loss after 168h salt spray test (B).
[0026] Fig. 9 Pull-off test of WPU samples composed of different composite fillers: pure WPU (A), GO / WPU (B), GO / PA-AT / WPU (C) before 168h salt spray; pure WPU (D), GO / WPU (E), GO / PA-AT / WPU (F) after 168h salt spray.
[0027] Fig.10 Electrochemical performance test diagrams of WPU coating samples with different mass ratios of GO and PA-AT (1:1, 1:2, 1:3, 1:4, 1:5); (A) Nyquist diagram, (B) Bode impedance modulus diagram, and (C) Bode phase angle diagram.
[0028] Fig.11 Tafel plots of bare steel sheet, WPU, and WPU samples with different mass ratios of GO and PA-AT added.
[0029] Fig.12 Electrochemical performance test diagrams of GO / PA-AT coating samples with different addition amounts; (A) Nyquist diagram, (B) Bode impedance modulus diagram, and (C) Bode phase angle diagram.
[0030] Fig.13 Tafel plots of bare steel, WPU and WPU samples with different addition amounts of GO / PA-AT. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0032] Example 1. Preparation of graphene oxide-based waterborne polyurethane marine anticorrosion coating 1. Preparation of tripolyaniline Dissolve p-phenylenediamine sulfate and aniline in HCl aqueous solution, and add ammonium persulfate. After stirring at room temperature for 1 hour, collect the resulting precipitate by filtration and wash with HCl aqueous solution. The solid product is washed with ammonia water and then rinsed with a large amount of distilled water, and then dried in a vacuum oven at 60°C overnight. The obtained aniline trimer (AT) is a purple-red solid.
[0033] 2. Preparation of phytic acid-doped polyaniline (PA-AT) AT and phytic acid (PA) were mixed in a mass ratio of 1:1, 1:2, 1:3, 1:4, 1:5, preferably 1:2, and ultrasonicated for 30 min at room temperature. The resulting precipitate was collected by filtration, and the solid product was washed with distilled water, and then dried in a vacuum oven at 60°C overnight.
[0034] 3. Preparation of graphene oxide / phytic acid-doped polyaniline (GO / PA-AT) Monolayer graphene oxide (GO) and PA-AT were mixed in mass ratios of 1:1, 1:2, 1:3, 1:4, and 1:5, preferably in a mass ratio of 1:3, and added into deionized water. After ultrasonic treatment for 1 hour, a uniformly dispersed GO / PA-AT mixed solution was obtained.
[0035] 4. Preparation of GO / PA-AT water-based composite coating 10mL GO / PA-AT dispersion (the weight of GO / PA-AT is 0.4g~1.2g) was mixed with 2.85g waterborne polyurethane curing agent and stirred at high speed for 10 minutes, and then added to waterborne polyurethane (WPU) (the amount of curing agent is 3wt% of WPU). The mixture was emulsified into a uniform emulsion under high-speed stirring for 10 minutes. Finally, the emulsion was sprayed on the treated Q235 carbon steel surface using an electric spray gun and then dried at room temperature for 7 days. The thickness of the coating is about 30µm. The main coating preparation process is as follows Figure 1 shown.
[0036] Example 2: Elemental analysis of graphene oxide-based waterborne polyurethane marine anticorrosion coating Figure 2 The infrared spectra of the intermediate products triphenylamine (AT) and phytated triphenylamine (PA-AT) in the synthesis process of composite fillers are shown at 612 cm -1 、932cm -1 and 1618cm -1 Characteristic peaks appeared at three positions, representing the bending vibration of PO, the symmetric vibration of POC and the stretching vibration of P=O, indicating that phytic acid was successfully doped onto triphenylamine.
[0037] Figure 3 The XPS element spectra, C1S spectra and N1s spectra of the materials at different stages in the synthesis of the composite filler. Figure 3 In (A), it can be observed that GO has two obvious peaks (C1s and O1s). Figure 3 , (A) In the XPS spectrum of GO / PA-AT, in addition to the C1s and O1s signal peaks, there are also N1s signal peaks and a weak P1p signal peak produced by doping with phytic acid. The C1s spectrum of GO is shown in Figure 1. Figure 3 , as shown in (B), the C1s signal of GO can be divided into three peaks with bond energies of 284.8 eV, 286.0 eV and 288.4 eV, corresponding to the CO bond, C=O bond and C=C bond, respectively. Figure 3 , (C) is the C1s spectrum of GO / PA-AT, which can be divided into four peaks, namely, CO bond (284.8 eV), C=O bond (286.6 eV), CN bond (287.1 eV) and C=C (288.5 eV). Figure 3, (D) is the N1s spectrum of GO / PA-AT. The analysis shows that the N1s signal of GO / PA-AT can be divided into three peaks, corresponding to three types of N, -N= (398.7eV) quinone imine and -NH- (400.2eV) phenylenediamine, indicating the formation of AT molecular chains; the polaron state (401.9eV) indicates the presence of PA doping sites N + XPS analysis further proved that PA was successfully doped onto AT.
[0038] Example 3: Morphology Analysis of Graphene Oxide-Based Waterborne Polyurethane Marine Anticorrosion Coating Figure 4 The morphology and structure of three samples, GO, PA-AT and GO / PA-AT, are shown. Figure 4 , (A) It can be seen that GO has a lamellar structure with a smooth surface and slight wrinkles. Figure 4 , (B) is the SEM image of phytic acid-doped trianiline, showing irregular spherical nanoparticles with irregular aggregation morphology and loose arrangement. Figure 4 As shown in (C), compared with GO alone, in the GO / PA-AT composite material, PA-AT is dispersed on the surface of graphene oxide sheets in the form of spheres of different sizes, forming a rough surface and a large area of wrinkled structure. The rough surface is more conducive to the dispersion of nanomaterials in the waterborne polyurethane matrix.
[0039] Example 4: Electrochemical performance analysis of graphene oxide-based waterborne polyurethane marine anticorrosion coating AC impedance and polarization curve tests were used to evaluate the corrosion resistance of coatings with different additives dispersed in 3.5wt%NaCl solution. Figure 5 The Nyquist diagram, Bode impedance modulus diagram, and Bode phase angle diagram are shown respectively. The impedance spectrum of the WPU coating changes significantly with the addition of different additives. In the Nyquist diagram, the capacitance arc and the diameter of the coating system are used as the criteria for evaluating the corrosion resistance of the coating, that is, the larger the diameter of the semicircular arc, the better the corrosion protection performance of the coating. Figure 5 , (A) It can be seen that in the Nyquist diagram, whether compared with bare steel, pure WPU coating or GO / WPU coating, the WPU coating with GO / PA-AT composite material has the largest arc diameter. In the Bode phase angle diagram, due to the pure resistance characteristics of the coating, the phase angle will show a close to 90°. As the electrolyte solution gradually penetrates into the coating, due to the parallel capacitance characteristics of the coating, the phase angle at a given frequency decreases. The change in phase angle may reflect the performance of the coating. In the Bode impedance modulus diagram, in the low frequency region (Zf=10 -2 The larger the impedance modulus at Hz, the better the anti-corrosion performance of the coating. Figure 5In (B), compared with other coating samples, the experimental group with GO / PA-AT composite material has the largest impedance modulus in the low-frequency region. In the Bode phase angle diagram, compared with other coating samples, the experimental group with GO / PA-AT composite material has the largest phase angle in the high-frequency region. The maximum phase angle is close to 90°, indicating that the passivation film is intact, and the smaller it is, the poorer the integrity. At the same time, Figure 5 , (B) and (C) Bode plots also confirm this conclusion. Therefore, the experimental group with GO / PA-AT composite material shows the best anti-corrosion performance.
[0040] Figure 6 The Tafel curve obtained from the polarization curve test is shown in Table 1. At the same time, the anti-corrosion efficiency is used to further evaluate the corrosion resistance of the waterborne composite coating. The anti-corrosion efficiency value is calculated according to the following formula: i 0 corr represents the corrosion current density of the bare carbon steel electrode, i corr Represents the corrosion current density of the coating.
[0041] Table 1 Polarization data of coatings made with different composite fillers Ecorr(mV) icorr (μA / cm2) ƞ(%) Bare -0.847 1.254×10-5 / WPU -0.594 1.972×10-6 84.27 GO / WPU -0.572 9.334×10-7 92.56 GO / PA-AT / WPU -0.001 1.254×10-8 99.90 Example 5: Mechanical properties analysis of graphene oxide-based waterborne polyurethane marine anticorrosion coating Figure 7 The results of mechanical property tests of the prepared coatings. Compared with pure WPU coatings, both GO / WPU coatings and GO / PA-AT / WPU coatings exhibit better impact resistance. A weight of uniform specifications was dropped from a height of 50 cm to measure its impact resistance. The results show that no obvious cracks appeared in the dented parts of the GO / WPU and GO / PA-AT / WPU coatings, which may be related to the huge layered structure of GO and GO / PA-AT, which can absorb impact energy. However, for pure WPU coatings, cracks will appear when the drop height exceeds 40 cm. Overall, after hardness, adhesion and impact resistance tests, the GO / PA-AT / WPU coating samples exhibited excellent performance. In addition, various mechanical property tests were carried out on WPU coating specimens with different mass ratios. Such as Figure 7 As shown in (F), the hardness value of the pure WPU sample is 2H (generally, the higher the H value, the higher the hardness). It can be seen that the addition of graphene oxide / PA-AT composite materials can improve the hardness of the coating. When the mass ratio of graphene oxide to PA-AT is 1:3, the H value of the coating can reach 4.
[0042] Adhesion test was carried out during the neutral salt spray test, and the results were as follows Figure 8As shown. Before the neutral salt spray test, the adhesion of the pure WPU coating reached 2.13MPa. With the addition of graphene oxide, its adhesion increased to 2.86MPa. More importantly, the WPU coating with GO / PA-AT added had the highest adhesion of 3.57MPa. Figure 8 , (B) It can be seen that the sample coated with GO / PA-AT / WPU coating has the smallest adhesion loss of 38%, while the adhesion losses of pure WPU coating and GO / WPU coating are 60% and 55%, respectively.
[0043] After 168h of neutral salt spray test, the pull-off test results of different coatings are as follows: Fig. 9 As shown. After the pull-off test in the pure WPU coating sample, severe corrosion occurred on the carbon steel surface, and the coating was completely separated from the carbon steel substrate. In addition, the graphene oxide / water-based polyurethane sample had fewer corrosion products. In contrast, the GO / PA-AT / WPU coating can still maintain an adhesion of 2MPa after the salt spray test, which has been proven to have a good protective effect on the carbon steel substrate. This phenomenon may be due to the fact that the addition of GO / PA-AT composite materials increases the density of the coating, and the complex formed by PA and iron ions can greatly enhance the adhesion of the functional coating on the surface of the metal sample.
[0044] Example 6. Optimization of the mass ratio of graphene oxide (GO) and phytic acid-doped triphenylamine (PA-AT) Fig.10 The electrochemical performance test diagrams of bare steel sheet, WPU and WPU samples with different mass ratios of GO and PA-AT (1:1, 1:2, 1:3, 1:4, 1:5) are shown. Fig.10 , A), compared with other experimental groups, when the mass ratio of GO to PA-AT is 1:3, the arc diameter of the WPU coating of the composite material is the largest. In the Bode impedance modulus diagram ( Fig.10 , B), compared with other coating samples, the experimental group of composite materials with a mass ratio of GO and PA-AT of 1:3 has the largest impedance modulus in the low-frequency region. In the Bode phase angle diagram, compared with other coating samples, the experimental group of composite materials with a mass ratio of GO and PA-AT of 1:3 has the largest phase angle in the high-frequency region. The maximum phase angle is close to 90°, indicating that the passivation film is intact, and the smaller it is, the poorer the integrity. Therefore, the experimental group of composite materials with a mass ratio of GO and PA-AT of 1:3 has the best anti-corrosion performance. At the same time, Fig.10 ,The Bode plots of (B) and (C) also confirm this conclusion.,Therefore, when the mass ratio of GO and PA-AT is 1:3, the waterborne polyurethane coating has the best anti-corrosion performance.
[0045] Polarization curves are also used to reveal the corrosion resistance of waterborne composite coatings in 3.5wt% NaCl solution. After AC impedance test, Tafel plots and polarization data of different coating samples (bare steel, WPU and adding different mass ratios of GO and PA-AT (1:1, 1:2, 1:3, 1:4, 1:5) are shown in Figure 2. Fig.11 And as shown in Table 2.
[0046] Table 2 Polarization data of bare steel, WPU, and WPU coatings with different mass ratios of GO and MP Ecorr(mV) icorr(μA / cm) ƞ(%) Bare -0.847 1.254×10-5 / WPU -0.594 1.972×10-6 84.27 1:1 -0.442 1.285×10-7 98.98 1:2 -0.057 4.118×10-8 99.67 1:3 0.023 2.752×10-8 99.78 1:4 -0.399 6.813×10-8 99.46 1:5 -0.564 3.860×10-7 96.85 Example 7: Effect of the amount of graphene oxide / phytic acid-doped triphenylamine (GO / PA-AT) added on the anticorrosion performance of waterborne polyurethane coating When the optimal mass ratio of GO and PA-AT was 1:3, the effects of different addition amounts of GO / PA-AT on the anti-corrosion performance of waterborne polyurethane coatings were investigated. Fig.12 The electrochemical performance test graphs of bare steel sheet, WPU and WPU coating with different addition amounts of GO / PA-AT (0.4g, 0.6g, 0.8g, 1g, 1.2g) are shown.
[0047] Polarization curves are also used to reveal the corrosion resistance of waterborne composite coatings in 3.5wt% NaCl solution. After AC impedance test, the Tafel plots and polarization data of different coating samples with different addition amounts of GO / PA-AT (0.4g, 0.6g, 0.8g, 1g, 1.2g) are shown in Figure 2. Fig.13 And as shown in Table 3.
[0048] Table 3 Polarization curves of bare steel, WPU and WPU samples with different addition amounts of GO / PA-AT Ecorr(mV) icorr(μA / cm) ƞ(%) Bare -0.847 1.254×10-5 / WPU -0.594 1.972×10-6 84.27 0.4g -0.432 1.412×10-7 98.87 0.6g -0.138 4.319×10-8 99.66 0.8g 0.023 2.752×10-8 99.78 1g -0.068 3.518×10-8 99.72 1.2g -0.493 4.444×10-7 96.46 The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a graphene oxide-based waterborne polyurethane marine anticorrosion coating, It is characterized in that The preparation steps include: (1) Preparation of phytic acid-doped triphenylamine The tripolyaniline and phytic acid are mixed, ultrasonicated at room temperature for 30 minutes, the resulting precipitate is collected by filtration, the solid product is washed with distilled water, and then dried to obtain the product; (2) Preparation of graphene oxide / phytic acid-doped triphenylamine Graphene oxide and phytic acid-doped triphenylamine were mixed and added into deionized water, and then ultrasonicated for 1 h to obtain a uniformly dispersed GO / PA-AT mixed solution; (3) Preparation of GO / PA-AT water-based composite coating The GO / PA-AT mixed liquid was mixed with the waterborne polyurethane curing agent and stirred at high speed for 10 minutes, then added into the waterborne polyurethane solution and emulsified into a uniform emulsion under high-speed stirring for 10 minutes to obtain a graphene oxide-based waterborne polyurethane marine anticorrosive coating material.
2. The method according to claim 1, It is characterized in that The method also includes the steps of preparing tripolyaniline: dissolving p-phenylenediamine sulfate and aniline in an aqueous solution of HCl, adding ammonium persulfate, stirring at room temperature for 1 hour, collecting the obtained precipitate by filtration and washing it with an aqueous solution of HCl, washing the solid product with ammonia water and then with a large amount of distilled water, and then drying it at 60°C.
3. The method according to claim 1, It is characterized in that In step (1), the mass ratio of tripolyaniline and phytic acid when mixed is 1:1-5.
4. The method according to claim 3, It is characterized in that In step (1), the mass ratio of trianiline and phytic acid when mixed is 1:
2.
5. The method according to claim 1, It is characterized in that In step (2), the mass ratio of graphene oxide to phytic acid-doped triphenylamine is 1:1-5.
6. The method according to claim 5, It is characterized in that In step (2), the mass ratio of graphene oxide to phytic acid-doped triphenylamine is 1:
3.
7. The method according to claim 1, It is characterized in that In step (3), the mass ratio of GO / PA-AT to waterborne polyurethane is 0.4~1.2:
95.
8. The method according to claim 1, It is characterized in that In step (3), the mass ratio of GO / PA-AT to waterborne polyurethane is 0.8:
95.
9. The method according to claim 5, It is characterized in that In step (3), the amount of waterborne polyurethane curing agent used is 3wt% of the waterborne polyurethane.
Citation Information
Cited By
Environment-adaptive high-energy-absorption intelligent anticorrosive coating and preparation method thereof
CN122255854A