High-strength flame-retardant polyurethane material and preparation method thereof

Through the synergistic effect of preparing composite reinforced fibers and using flame retardants such as ammonium polyphosphate, barium phytate, chitosan, etc., the problems of mechanical properties of polyurethane materials deteriorated and environmental pollution after adding flame retardants are solved, and high strength and Polyurethane material with good flame retardancy.

CN119039764AInactive Publication Date: 2024-11-29SHANGHAI JIELI NEW MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411514422.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The addition of added flame retardants in the curing and forming process of existing polyurethane materials will affect their mechanical properties and will migrate over time, which poses the potential risk of polluting the environment, making it difficult to have good flame retardancy and high strength at the same time.

Method used

By preparing composite reinforced fibers, including calcium alginate, aramid and montmorillonite, combined with the synergistic effects of ammonium polyphosphate, barium phytate and chitosan, a high-strength flame retardant polyurethane materials are formed, utilizing the structural characteristics of the fiber and flame retardant. The synergistic mechanism of agents improves the flame retardant properties and strength of the material.

Benefits of technology

Polyurethane materials with high strength and good flame retardancy have been achieved. Through the synergistic action of composite fibers and flame retardants, the flame retardant and mechanical properties of the material are significantly improved and the risk of environmental pollution is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a high-strength flame-retardant polyurethane material and a preparation method thereof, and belongs to the technical field of polyurethane materials. Comprising the following raw materials in parts by weight: 90-110 parts of polyol, 50-65 parts of isocyanate, 15-20 parts of a flame retardant, 5-8 parts of composite reinforced fibers, 12-17 parts of a chain extender and 1-1.5 parts of a catalyst, the strength of the polyurethane material is improved through reaction of polyol and isocyanate and addition of composite reinforced fibers, the flame retardant keeps excellent flame retardance through compounding of ammonium polyphosphate, barium phytate and chitosan, then the chain extender and the catalyst are added, and the polyurethane material with high strength and good flame retardance is prepared through vulcanization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials and relates to a high-strength flame-retardant polyurethane material and a preparation method thereof. Background Art

[0002] Polyurethane is a type of polymer with a main chain containing -NHCOO- repeating structural units. It is formed by the polymerization of isocyanate (monomer) and hydroxyl compounds. Because it contains highly polar urethane groups, it is insoluble in non-polar solvents and has good oil resistance, toughness, wear resistance, aging resistance, etc. It is widely used in home furnishing, construction, daily necessities, transportation, home appliances, etc.

[0003] Adding some additive flame retardants during the curing process of polyurethane materials will have an adverse effect on the mechanical properties of the polyurethane materials. Moreover, as time goes by, the additive flame retardants will migrate, posing a potential risk of environmental pollution.

[0004] Therefore, it is necessary to develop a polyurethane material that has both good flame retardancy and good strength. Summary of the invention

[0005] The purpose of the present invention is to provide a high-strength flame-retardant polyurethane material and a preparation method thereof. The polyurethane material prepared by the present invention has high strength and good flame retardancy.

[0006] The purpose of the present invention can be achieved through the following technical solutions: A high-strength flame-retardant polyurethane material comprises the following raw materials in parts by weight: 90-110 parts of polyol, 50-65 parts of isocyanate, 15-20 parts of flame retardant, 5-8 parts of composite reinforcing fiber, 12-17 parts of chain extender and 1-1.5 parts of catalyst; Among them, the preparation process of the composite reinforced fiber is as follows: S1.1. Sodium alginate and deionized water are mixed in a mass ratio of 1:10 to obtain a mixed solution A, sodium hydroxide is added to adjust the pH of the mixed solution A to 8-10, calcium chloride (5-10% by mass of the sodium alginate) is added at 50-65°C and stirred for 3-5 hours, after the stirring is completed, the solid is collected by filtration and dried at 80-90°C for 10 hours to obtain calcium alginate solid; S1.2. Calcine montmorillonite in a muffle furnace at a temperature of 500°C for 2-3 hours, grind the aramid and the calcined montmorillonite by a ball mill at a speed of 500-600 r / min for 3-5 hours, and then pass through a 200-mesh sieve to obtain aramid powder and montmorillonite powder, stir the calcium alginate solid, aramid powder and montmorillonite powder for 15-20 minutes, melt at 170-190°C for 1-1.5 hours, and then melt-spin in a melt spinning machine at a temperature of 220-240°C, control the spinning rate to 700-800 m / min, and stretch after spinning, control the stretch ratio to 3-4 times, to obtain the composite reinforced fiber.

[0007] As a preferred technical solution of the present invention, in step S1.2, the mass ratio of the calcium alginate solid, the aramid powder and the montmorillonite powder is (20-35): (5-10): (5-10).

[0008] As a preferred technical solution of the present invention, the preparation process of the flame retardant is as follows: S3.1. In parts by weight, at 30-35°C, 10-15 parts of barium carbonate are dispersed in 80-100 parts of deionized water to prepare a suspension A, and 10-15 parts of phytic acid are dissolved in 50-60 parts of deionized water to obtain a phytic acid solution. The phytic acid solution and the suspension A are mixed and stirred for 3-5 hours. After the stirring is completed, the mixture is filtered and washed with deionized water for 5 times. The collected solid is dried at 75-80°C for 10-14 hours to obtain a barium phytate solid. S3.2. Stir ammonium polyphosphate and barium phytate in a mass ratio of (3-5):1 for 20-30 min at a stirring speed of 300-400 r / min to obtain a mixture C. Mix chitosan with 0.2 mol / L phosphoric acid solution to obtain a chitosan dispersion. Add mixture C to the chitosan dispersion at 60-70°C, wherein the mass ratio of mixture C to chitosan dispersion is 1:(10-15). Maintain the stirring speed for 1-3 h. After cooling, let stand for 1 h. Dry at 100-110°C for 10 h to obtain the flame retardant.

[0009] As a preferred technical solution of the present invention, the catalyst is one of diisobutyltin dilaurate, stannous octoate and stannous oleate.

[0010] As a preferred technical solution of the present invention, the chain extender is 1,4-butanediol.

[0011] As a preferred technical solution of the present invention, the polyol is one of polyethylene glycol, polypropylene glycol and polytetrahydrofuran diol.

[0012] As a preferred technical solution of the present invention, in step S3.2, the solid-liquid ratio of the chitosan to the 0.2 mol / L phosphoric acid solution is (3-5):100 g / mL.

[0013] A method for preparing a high-strength flame-retardant polyurethane material comprises the following preparation steps: S1. According to the weight ratio, the polyol is kept at 100-120°C for 2 hours, cooled to 65-75°C, and isocyanate is added under nitrogen and stirred for 2-4 hours to obtain a polyurethane matrix; S2, uniformly dispersing the composite reinforcing fiber and the flame retardant in the silane coupling agent solution, ultrasonically treating for 20-35 minutes, filtering to obtain a mixture, and drying the mixture at 75-85°C for 2-5 hours to obtain a mixed solid, wherein the solid-liquid ratio of the composite reinforcing fiber, the flame retardant and the silane coupling agent solution is 1:1:20 g / mL; S3, first add the mixed solid into the polyurethane matrix and stir evenly, then add the chain extender and the catalyst, stir for 10 to 20 minutes to mix evenly, and obtain a flame retardant polyurethane material; S4, pouring the flame-retardant polyurethane material on a flat vulcanizer at 110° C. for compression molding, and naturally cooling it to room temperature to prepare the high-strength flame-retardant polyurethane material.

[0014] As a preferred technical solution of the present invention, in step S2, the silane coupling agent solution is one of KH550 or KH560 solutions with a mass fraction of 10-18%.

[0015] As a preferred technical solution of the present invention, in step S4, the compression molding condition is to maintain a pressure of 10-15 MPa for 20-35 minutes.

[0016] In the present invention, the composite reinforcing fiber is prepared by calcium alginate, aramid and montmorillonite. Calcium alginate is composed of alginic acid and calcium ions, and its molecular structure has strong stability and porosity, which helps to enhance its flame retardant performance. When calcium alginate is heated, the hydroxyl and carboxyl groups in its molecular structure undergo a dehydration reaction to produce lactone substances, which can dilute the combustible gas to achieve a flame retardant effect. At the same time, montmorillonite can slow down the combustion speed by forming a barrier layer, absorbing heat, releasing water vapor, etc., so the composite reinforcing fiber also has a certain flame retardancy.

[0017] Calcium alginate is generated by reacting sodium alginate with calcium salt, and the composite fiber composed of calcium alginate, aramid fiber and montmorillonite is used to complement each other in fiber characteristics. Calcium alginate fiber has excellent biocompatibility and degradability, and aramid fiber has high strength and can significantly enhance the strength of the composite fiber. During the calcination process, the moisture and other volatiles between the montmorillonite layers are removed, so that the interlayer spacing is increased, the specific surface area is increased, and the structural stability of montmorillonite is improved by removing the unstable components in montmorillonite, so that it can still maintain good performance under high temperature or harsh environment. And through calcination treatment, the bonding force between montmorillonite particles is enhanced, thereby improving its mechanical strength, and the gap between fibers can be filled when preparing composite reinforced fibers, improving the bonding force between fibers, and further enhancing the strength of composite fibers. Adding composite reinforced fibers to polyurethane can bear part of the stress, thereby dispersing stress concentration, and therefore can improve the strength of polyurethane materials.

[0018] Barium phytate can melt and decompose into unstable gaseous oxides and fluid glassy substances at high temperatures. These products form a flame retardant layer that is difficult to penetrate on the burning surface, effectively preventing the spread of gas, smoke and flames. Barium phytate is prepared using barium carbonate and phytic acid. After ammonium polyphosphate and barium phytate are evenly mixed in a chitosan dispersion, chitosan forms a viscous film-forming solution through intramolecular and intermolecular hydrogen bonds, and forms a film after drying. Therefore, the film-forming property of chitosan can be evenly mixed with ammonium polyphosphate and barium phytate, and the compatibility with polyurethane is improved due to the chitosan treatment.

[0019] Chitosan, ammonium polyphosphate and barium phytate can produce a synergistic effect after compounding, making the overall flame retardant performance better than a single component. Ammonium polyphosphate and chitosan have flame retardant properties, and the addition of barium phytate further enhances this effect. This synergistic effect works together through different flame retardant mechanisms. Ammonium polyphosphate and chitosan produce flame retardant gases such as nitrogen and phosphoric acid during combustion, while barium phytate forms a flame retardant layer that is difficult to penetrate, jointly preventing the spread of flames. This synergistic effect can further enhance the flame retardant properties of polyurethane.

[0020] Beneficial effects of the present invention: The present invention improves the strength of the polyurethane material by reacting polyol with isocyanate and adding composite reinforcing fibers, and maintains excellent flame retardancy of the flame retardant by compounding ammonium polyphosphate, barium phytate and chitosan, and then adds a chain extender and a catalyst to prepare a polyurethane material with high strength and good flame retardancy through vulcanization. DETAILED DESCRIPTION

[0021] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0022] In the following examples and comparative examples: Sodium alginate: purchased from Wuhan Jiyesheng Chemical Co., Ltd.; Calcium chloride: purchased from Wuhan Jixinyibang Biotechnology Co., Ltd.; Montmorillonite: purchased from Wuhan Xinyang Ruihe Chemical Technology Co., Ltd.; Aramid: purchased from Dongguan Langfeng Plastic Raw Materials Co., Ltd., brand: WAL34; Barium carbonate: purchased from Wuhan Jiyesheng Chemical Co., Ltd.; Phytic acid: purchased from Nanjing Jingzhu Biotechnology Co., Ltd., purity 70%; Ammonium polyphosphate: purchased from Hubei Jusheng Technology Co., Ltd.; Chitosan: purchased from Shandong Fengtai Biotechnology Co., Ltd.; Polyethylene glycol: purchased from Jinan Huasheng Chemical Co., Ltd. Isocyanate: purchased from Shenyang Elex Chemical Co., Ltd. 1,4-Butanediol: purchased from Hubei Guangao Biotechnology Co., Ltd.; Stannous octoate: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: T818482; Polytetrahydrofurandiol: purchased from Hubei Yongkuo Technology Co., Ltd.; KH550: purchased from Shanghai Yuanye Biotechnology Co., Ltd.

[0023] Example 1 Preparation of composite reinforcing fibers: S1.1. Sodium alginate and deionized water in a mass ratio of 1:10 are mixed to obtain a mixed solution A, sodium hydroxide is added to adjust the pH of the mixed solution A to 8, calcium chloride (5% by mass of the sodium alginate) is added at 50°C and stirred for 3 hours, after the stirring is completed, the solid is collected by filtration and dried at 80°C for 10 hours to obtain calcium alginate solid; S1.2. Calcine montmorillonite in a muffle furnace at a temperature of 500°C for 2 hours, then grind the aramid and the calcined montmorillonite by a ball mill at a speed of 500 r / min for 3 hours, and then pass through a 200-mesh sieve to obtain aramid powder and montmorillonite powder, stir the calcium alginate solid, aramid powder and montmorillonite powder for 15 minutes, melt at 170°C for 1 hour, and then melt-spin in a melt spinning machine at a temperature of 220°C and a spinning rate of 700 m / min. After spinning, stretch the fibers and control the stretch ratio to 3 times to obtain the composite reinforced fiber; wherein the mass ratio of calcium alginate solid, aramid powder and montmorillonite powder is 20:5:5.

[0024] Preparation of flame retardant: S3.1. In parts by weight, at 30°C, 10 parts of barium carbonate are dispersed in 80 parts of deionized water to obtain a suspension A, and 10 parts of phytic acid are dissolved in 50 parts of deionized water to obtain a phytic acid solution. The phytic acid solution and the suspension A are mixed and stirred for 3 hours. After the stirring is completed, the mixture is filtered and washed with deionized water for 5 times. The collected solid is dried at 75°C for 10 hours to obtain a barium phytate solid. S3.2. Stir ammonium polyphosphate and barium phytate in a mass ratio of 3:1 for 20 minutes at a stirring speed of 300 r / min to obtain a mixture C. Mix chitosan with 0.2 mol / L phosphoric acid solution to obtain a chitosan dispersion. Add mixture C to the chitosan dispersion at 60°C, wherein the mass ratio of mixture C to chitosan dispersion is 1:10. Maintain the speed and continue stirring for 1 hour. After cooling, let it stand for 1 hour. Dry it at 100°C for 10 hours to obtain the flame retardant, wherein the solid-liquid ratio of chitosan to 0.2 mol / L phosphoric acid solution is 3:100 g / mL.

[0025] Preparation of high-strength flame-retardant polyurethane materials: S1. Preserve 90 parts of polyethylene glycol at 100°C for 2 hours, cool to 65°C, add 50 parts of isocyanate and stir for 2 hours under nitrogen to obtain a polyurethane matrix; S2, 5 parts of composite reinforcing fiber and 15 parts of flame retardant are uniformly dispersed in a KH550 solution with a mass fraction of 10%, and ultrasonically treated for 20 minutes. After completion, the mixture is filtered to obtain a mixture, and the mixture is dried at 75°C for 2 hours to obtain a mixed solid, wherein the solid-liquid ratio of the composite reinforcing fiber, the flame retardant and the silane coupling agent solution is 1:1:20 g / mL; S3, first add the mixed solid to the polyurethane matrix and stir evenly, then add 12 parts of 1,4-butanediol and 1 part of stannous octoate, stir for 10 minutes to mix evenly, and obtain a flame retardant polyurethane material; S4. Cast the flame-retardant polyurethane material on a flat vulcanizer at 110° C., maintain it at a pressure of 10 MPa for 20 minutes for compression molding, and naturally cool it to room temperature to prepare the high-strength flame-retardant polyurethane material.

[0026] Example 2 Preparation of composite reinforcing fibers: S1.1. Sodium alginate and deionized water in a mass ratio of 1:10 are mixed to obtain a mixed solution A, sodium hydroxide is added to adjust the pH of the mixed solution A to 9, calcium chloride (8% by mass of the sodium alginate) is added at 58°C and stirred for 4 hours, after the stirring is completed, the solid is collected by filtration and dried at 85°C for 10 hours to obtain calcium alginate solid; S1.2. Calcine montmorillonite in a muffle furnace at a temperature of 500°C for 2.5 hours, then grind the aramid and the calcined montmorillonite by a ball mill at a speed of 550 r / min for 4 hours, and then pass through a 200-mesh sieve to obtain aramid powder and montmorillonite powder, stir the calcium alginate solid, aramid powder and montmorillonite powder for 17 minutes, melt at 180°C for 1.2 hours, and then melt-spin in a melt spinning machine at a temperature of 230°C and a spinning rate of 750 m / min. After spinning, stretch it and control the stretch ratio to 3.5 times to obtain the composite reinforced fiber; wherein the mass ratio of calcium alginate solid, aramid powder and montmorillonite powder is 25:8:8.

[0027] Preparation of flame retardant: S3.1. In parts by weight, at 33°C, 12 parts of barium carbonate are dispersed in 90 parts of deionized water to prepare a suspension A, and 13 parts of phytic acid are dissolved in 55 parts of deionized water to obtain a phytic acid solution. The phytic acid solution and the suspension A are mixed and stirred for 4 hours. After the stirring is completed, the mixture is filtered and washed with deionized water for 5 times. The collected solid is dried at 77°C for 12 hours to obtain a barium phytate solid. S3.2. Stir ammonium polyphosphate and barium phytate in a mass ratio of 4:1 for 25 minutes at a stirring speed of 350 r / min to obtain a mixture C. Mix chitosan with 0.2 mol / L phosphoric acid solution to obtain a chitosan dispersion. Add mixture C to the chitosan dispersion at 65°C, wherein the mass ratio of mixture C to chitosan dispersion is 1:12. Maintain the speed and continue stirring for 2 hours. After cooling, let it stand for 1 hour. Dry it at 105°C for 10 hours to obtain the flame retardant, wherein the solid-liquid ratio of chitosan to 0.2 mol / L phosphoric acid solution is 4:100 g / mL.

[0028] Preparation of high-strength flame-retardant polyurethane materials: S1. Keep 100 parts of polyethylene glycol at 110° C. for 2 hours, cool to 70° C., add 58 parts of isocyanate and stir for 3 hours under nitrogen to obtain a polyurethane matrix; S2, 6 parts of composite reinforcing fiber and 18 parts of flame retardant are uniformly dispersed in a KH550 solution with a mass fraction of 15%, and ultrasonically treated for 28 minutes. After completion, the mixture is filtered to obtain a mixture, and the mixture is dried at 80°C for 4 hours to obtain a mixed solid, wherein the solid-liquid ratio of the composite reinforcing fiber, the flame retardant and the silane coupling agent solution is 1:1:20 g / mL; S3, first add the mixed solid to the polyurethane matrix and stir evenly, then add 15 parts of 1,4-butanediol and 1.3 parts of stannous octoate, stir for 15 minutes to mix evenly, and obtain a flame retardant polyurethane material; S4. Cast the flame-retardant polyurethane material on a flat vulcanizer at 110° C., maintain it at a pressure of 13 MPa for 28 minutes for compression molding, and naturally cool it to room temperature to prepare the high-strength flame-retardant polyurethane material.

[0029] Example 3 Preparation of composite reinforcing fibers: S1.1. Sodium alginate and deionized water in a mass ratio of 1:10 are mixed to obtain a mixed solution A, sodium hydroxide is added to adjust the pH of the mixed solution A to 10, calcium chloride (10% by mass of the sodium alginate) is added at 65°C and stirred for 5 hours, after the stirring is completed, the solid is collected by filtration and dried at 90°C for 10 hours to obtain calcium alginate solid; S1.2. Calcine montmorillonite in a muffle furnace at a temperature of 500°C for 3 hours, then grind the aramid and the calcined montmorillonite by a ball mill at a speed of 600 r / min for 5 hours, and then pass through a 200-mesh sieve to obtain aramid powder and montmorillonite powder, stir the calcium alginate solid, aramid powder and montmorillonite powder for 20 minutes, melt them at 190°C for 1.5 hours, and then melt-spin them in a melt spinning machine at a temperature of 240°C and a spinning rate of 800 m / min. After spinning, draw the fibers and control the draw ratio to 4 times to obtain the composite reinforced fiber; wherein the mass ratio of calcium alginate solid, aramid powder and montmorillonite powder is 35:10:10.

[0030] Preparation of flame retardant: S3.1, in parts by weight, at 35°C, 15 parts of barium carbonate are dispersed in 100 parts of deionized water to prepare a suspension A, and 15 parts of phytic acid are dissolved in 60 parts of deionized water to obtain a phytic acid solution, the phytic acid solution and the suspension A are mixed and stirred for 5 hours, after the stirring is completed, the mixture is filtered and washed with deionized water for 5 times, and the collected solid is dried at 80°C for 14 hours to obtain a barium phytate solid; S3.2. Stir ammonium polyphosphate and barium phytate in a mass ratio of 5:1 for 30 minutes at a stirring speed of 400 r / min to obtain a mixture C. Mix chitosan with 0.2 mol / L phosphoric acid solution to obtain a chitosan dispersion. Add mixture C to the chitosan dispersion at 70°C, wherein the mass ratio of mixture C to chitosan dispersion is 1:15. Maintain the speed and continue stirring for 3 hours. After cooling, let it stand for 1 hour. Dry it at 110°C for 10 hours to obtain the flame retardant, wherein the solid-liquid ratio of chitosan to 0.2 mol / L phosphoric acid solution is 5:100 g / mL.

[0031] Preparation of high-strength flame-retardant polyurethane materials: S1. By weight, 110 parts of polytetrahydrofuran diol were kept at 120° C. for 2 hours, cooled to 75° C., and 65 parts of isocyanate were added and stirred for 4 hours under nitrogen to obtain a polyurethane matrix; S2, 8 parts of composite reinforcing fiber and 20 parts of flame retardant are uniformly dispersed in a KH550 solution with a mass fraction of 18%, and ultrasonically treated for 35 minutes. After completion, the mixture is filtered to obtain a mixture, and the mixture is dried at 85°C for 5 hours to obtain a mixed solid, wherein the solid-liquid ratio of the composite reinforcing fiber, the flame retardant and the silane coupling agent solution is 1:1:20 g / mL; S3, first add the mixed solid to the polyurethane matrix and stir evenly, then add 17 parts of 1,4-butanediol and 1.5 parts of stannous octoate, stir for 10-20 minutes to mix evenly, and obtain a flame retardant polyurethane material; S4. Cast the flame-retardant polyurethane material on a flat vulcanizer at 110° C., maintain it at a pressure of 15 MPa for 35 minutes for compression molding, and naturally cool it to room temperature to prepare the high-strength flame-retardant polyurethane material.

[0032] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that aramid is not added during the preparation of the composite reinforcing fiber in Comparative Example 1, and the other operations are the same.

[0033] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that no montmorillonite is added during the preparation of the composite reinforcing fiber in Comparative Example 2, and the other operations are the same.

[0034] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that barium phytate is not added during the preparation of the flame retardant in Comparative Example 3, and the other operations are the same.

[0035] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that chitosan treatment is not performed during the preparation of the flame retardant in Comparative Example 4, and the other operations are the same.

[0036] Performance Test: 1. Flame retardancy: The polyurethane materials prepared in Examples 1-3 and Comparative Examples 1-4 were made into strips with a length of 130 mm, a width of 6.5 mm, and a thickness of 3 mm according to the standard GB / T 2408-2008. After curing for 7 days at a temperature of 23°C and a humidity of 50%, the limiting oxygen index of the sealing adhesive was tested using an oxygen index tester; the polyurethane materials prepared in Examples 1-3 and Comparative Examples 1-4 were tested for burning time according to GB 8624-2012. The specific results are shown in Table 1: Table 1

[0037] According to the data in Table 1, the limiting oxygen index obtained in Examples 1-3 is higher than that in Comparative Examples 1-4, and the average burning time and the peak heat release rate are significantly lower than those in Comparative Examples 1-4, so Examples 1-3 have better flame retardant properties.

[0038] 2. The mechanical properties of the polyurethane materials prepared in Examples 1-3 and Comparative Examples 1-4 were measured according to GB / T 528-2009. The results are shown in Table 2:

[0039] According to the data in Table 2, the tensile strength, compressive strength and elongation at break measured in Examples 1-3 are all higher than those in Comparative Examples 1-4. Therefore, the polyurethane materials prepared in Examples 1-3 have better mechanical properties and thus higher strength.

[0040] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A high-strength flame-retardant polyurethane material, characterized in that: The method comprises the following raw materials in parts by weight: 90 to 110 parts of polyol, 50 to 65 parts of isocyanate, 15 to 20 parts of flame retardant, 5 to 8 parts of composite reinforcing fiber, 12 to 17 parts of chain extender and 1 to 1.5 parts of catalyst; Among them, the preparation process of the composite reinforced fiber is as follows: S1.

1. Sodium alginate and deionized water are mixed in a mass ratio of 1:10 to obtain a mixed solution A, sodium hydroxide is added to adjust the pH of the mixed solution A to 8-10, calcium chloride (5-10% by mass of the sodium alginate) is added at 50-65°C and stirred for 3-5 hours, after the stirring is completed, the solid is collected by filtration and dried at 80-90°C for 10 hours to obtain calcium alginate solid; S1.

2. Calcine montmorillonite in a muffle furnace at a temperature of 500°C for 2-3 hours, grind the aramid and the calcined montmorillonite by a ball mill at a speed of 500-600 r / min for 3-5 hours, and then pass through a 200-mesh sieve to obtain aramid powder and montmorillonite powder, stir the calcium alginate solid, aramid powder and montmorillonite powder for 15-20 minutes, melt at 170-190°C for 1-1.5 hours, and then melt-spin in a melt spinning machine at a temperature of 220-240°C, control the spinning rate to 700-800 m / min, and stretch after spinning, control the stretch ratio to 3-4 times, to obtain the composite reinforced fiber.

2. The high-strength flame-retardant polyurethane material according to claim 1, characterized in that: In step S1.2, the mass ratio of the calcium alginate solid, the aramid powder and the montmorillonite powder is (20-35): (5-10): (5-10).

3. The high-strength flame-retardant polyurethane material according to claim 1, characterized in that: The preparation process of the flame retardant is as follows: S3.

1. In parts by weight, at 30-35°C, 10-15 parts of barium carbonate are dispersed in 80-100 parts of deionized water to prepare a suspension A, and 10-15 parts of phytic acid are dissolved in 50-60 parts of deionized water to obtain a phytic acid solution. The phytic acid solution and the suspension A are mixed and stirred for 3-5 hours. After the stirring is completed, the mixture is filtered and washed with deionized water for 5 times. The collected solid is dried at 75-80°C for 10-14 hours to obtain a barium phytate solid. S3.

2. Stir ammonium polyphosphate and barium phytate in a mass ratio of (3-5):1 for 20-30 min at a stirring speed of 300-400 r / min to obtain a mixture C. Mix chitosan with 0.2 mol / L phosphoric acid solution to obtain a chitosan dispersion. Add mixture C to the chitosan dispersion at 60-70°C, wherein the mass ratio of mixture C to chitosan dispersion is 1:(10-15). Maintain the stirring speed for 1-3 h. After cooling, let stand for 1 h. Dry at 100-110°C for 10 h to obtain the flame retardant.

4. The high-strength flame-retardant polyurethane material according to claim 1, characterized in that: The catalyst is one of diisobutyltin dilaurate, stannous octoate and stannous oleate.

5. The high-strength flame-retardant polyurethane material according to claim 1, characterized in that: The chain extender is 1,4-butanediol.

6. The high-strength flame-retardant polyurethane material according to claim 1, characterized in that: The polyol is one of polyethylene glycol, polypropylene glycol and polytetrahydrofuran diol.

7. The high-strength flame-retardant polyurethane material according to claim 3, characterized in that: In step S3.2, the solid-liquid ratio of the chitosan to the 0.2 mol / L phosphoric acid solution is (3-5):100 g / mL.

8. A method for preparing a high-strength flame-retardant polyurethane material according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: S1. According to the weight ratio, the polyol is kept at 100-120°C for 2 hours, cooled to 65-75°C, and isocyanate is added under nitrogen and stirred for 2-4 hours to obtain a polyurethane matrix; S2, uniformly dispersing the composite reinforcing fiber and the flame retardant in the silane coupling agent solution, ultrasonically treating for 20-35 minutes, filtering to obtain a mixture, and drying the mixture at 75-85°C for 2-5 hours to obtain a mixed solid, wherein the solid-liquid ratio of the composite reinforcing fiber, the flame retardant and the silane coupling agent solution is 1:1:20 g / mL; S3, first add the mixed solid into the polyurethane matrix and stir evenly, then add the chain extender and the catalyst, stir for 10 to 20 minutes to mix evenly, and obtain a flame retardant polyurethane material; S4, pouring the flame-retardant polyurethane material on a flat vulcanizer at 110° C. for compression molding, and naturally cooling to room temperature to prepare the high-strength flame-retardant polyurethane material.

9. The method for preparing a high-strength flame-retardant polyurethane material according to claim 8, characterized in that: In step S2, the silane coupling agent solution is one of KH550 or KH560 solutions with a mass fraction of 10-18%.

10. The method for preparing a high-strength flame-retardant polyurethane material according to claim 8, characterized in that: In step S4, the compression molding is performed under a pressure of 10-15 MPa for 20-35 min.

Citation Information

Patent Citations

  • Method for preparing selenium-enriched fiber

    CN105019050A

  • Flame-retardant polyester lining cloth and preparing method thereof

    CN106245145A

  • Biomass composite ammonium polyphosphate intumescent flame retardant, preparation method and application thereof

    CN112063019A

  • Composition for fiber surface treatment and fiber treatment method

    CN114341424A

  • Washable cold aiding agent and preparation method thereof

    CN117802613A

Cited By

  • Waterproof and breathable polyurethane film and preparation method thereof

    CN120648209A

  • Environment-friendly flame-retardant synthetic leather and production process thereof

    CN122326098A