Preparation method of polyphenol-modified vinyl POSS (Polyhedral Oligomeric Silsesquioxane) modified soybean protein adhesive
The preparation method of polyphenol-modified octavinyl POSS-modified soybean protein adhesive solves the problems of insufficient water resistance, flame retardancy and mildew resistance of soybean protein adhesive, and realizes the application of high-performance adhesive.
Patent Information
- Application Number
- CN202411011920.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
AI Technical Summary
Existing soybean protein adhesives have shortcomings in terms of water resistance, flame retardancy, and mildew resistance, which limits their application in the wood industry.
A method for preparing polyphenol-modified octavinyl POSS-modified soybean protein adhesive involves adding octavinyl POSS and borax to form a cross-linked network, thereby improving the adhesive's water resistance, flame retardancy, and mildew resistance.
It significantly improves the water resistance, bonding properties, flame retardancy, and mildew resistance of adhesives, meeting the requirements of industrial applications.
Smart Images

Figure CN118995129A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an adhesive, in particular to a method for preparing a polyphenol-modified vinyl POSS-modified soybean protein adhesive. Background Art
[0002] In the production and processing of wood-based panels, "trialdehyde glue" (mainly phenolic resin, urea-formaldehyde resin and melamine formaldehyde resin) is still the most widely used synthetic adhesive, especially urea-formaldehyde resin glue, which has the largest usage. This type of adhesive has a wide range of sources, has excellent bonding properties and high water resistance, but its raw materials usually come from non-renewable chemical resources such as petroleum, and will release toxic substances such as formaldehyde and phenol during production and use, causing great harm to human health. In the face of global climate change, in order to reduce the excessive dependence of the wood-based panel industry on fossil adhesives, it is urgent to develop a green, environmentally friendly, sustainable and environmentally friendly adhesive.
[0003] At present, bio-based wood adhesives have become a research hotspot as a natural, renewable and environmentally friendly adhesive. Biomass resources are widely available and inexpensive, and are a type of green and non-toxic natural polymer material. Many researchers use starch, protein, lignin and tannin to replace toxic phenol to make adhesives. Among them, soy protein adhesives have great application potential in the wood industry and agriculture because of their easy availability of raw materials, low production cost and biodegradability, and have good application prospects in replacing aldehyde adhesives for wood. However, soy protein adhesives have low bonding strength and poor water resistance, and are usually modified by chemical crosslinking, organic-inorganic, and biomimetic methods. Among them, chemical crosslinking modification is one of the most effective methods to improve the water-resistant bonding strength of soy protein adhesives. However, it is not enough for soy protein adhesives to only meet environmental protection requirements, and more performance needs to be explored on the basis of green and formaldehyde-free. Some researchers have studied the improvement of the flame retardancy of soy protein adhesives and found that while improving the flame retardancy, the bonding strength will decrease. Secondly, since soybean protein contains rich nutrients, it is easily attacked by microorganisms in a humid environment, causing soybean protein adhesives to mold and endanger human health. In view of the above problems, it is urgent to find a method to simultaneously improve the water resistance, flame retardancy and mildew resistance of soybean protein adhesives, so as to realize the industrial application of soybean protein adhesives. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a polyphenol-modified vinyl POSS-modified soybean protein adhesive. The polyphenol-modified vinyl POSS-modified soybean protein adhesive prepared by the present invention has high water-resistant bonding performance, flame retardancy and mildew resistance.
[0005] The technical solution of the present invention is a method for preparing a polyphenol-modified vinyl POSS-modified soybean protein adhesive, comprising the following steps:
[0006] S1. Extraction of urushiol:
[0007] a. Mixing raw lacquer and ethanol, and stirring until the raw lacquer is evenly dispersed in the ethanol to obtain a raw lacquer ethanol solution;
[0008] b. Filter the raw lacquer ethanol solution to obtain a clear lacquer phenol solution;
[0009] c. Rotary evaporation of the urushiol solution to remove ethanol to obtain a brown viscous liquid, which is urushiol;
[0010] S2, uniformly mixing urushiol, octavinyl POSS and ammonium persulfate to obtain POSS-U;
[0011] S3. Dissolve sodium dodecyl sulfate in water and adjust the pH to between 8 and 9. Then add POSS-U, soy protein isolate and borax and stir evenly to obtain a polyphenol-modified vinyl POSS modified soy protein adhesive.
[0012] In the above-mentioned method for preparing the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step a of step S1, the usage ratio of raw lacquer and ethanol is 1 g: 25-35 mL.
[0013] In the preparation method of the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step c of step S1, the rotary evaporation temperature is 45-55° C., and the rotary evaporation speed is 100-150 rpm.
[0014] In the preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive, in step S2, the mass ratio of urushiol to octavinyl POSS is 2-5:1-3, and the mass percentage of ammonium persulfate is 0.5-1.5%.
[0015] In the preparation method of the polyphenol-modified vinyl POSS modified soy protein adhesive, in step S2, the mass ratio of urushiol to octavinyl POSS is 3:2, and the mass of ammonium persulfate added is 1% of the total mass of urushiol and octavinyl POSS.
[0016] In the preparation method of the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step S3, the mass ratio of sodium dodecyl sulfate to water is 5-10:800-1000.
[0017] In the preparation method of the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step S3, the pH is adjusted by adding sodium hydroxide.
[0018] In the preparation method of the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step S3, the mass ratio of POSS-U, SPI and borax is 3:12:0.5-3.
[0019] In the above-mentioned method for preparing the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step S3, the mass ratio of POSS-U, SPI and borax is 3:12:1.5.
[0020] In the preparation method of the polyphenol-modified vinyl POSS-modified soybean protein adhesive, in step S3, the stirring speed is 400-450 rpm, and the stirring time is 20-30 min.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] Octavidinyl cage polysilsesquioxane (octavinyl POSS) is an organic-inorganic hybrid molecule with a nanostructure. Its organic groups are extensive, and the Si-O-Si structure in the compound has good thermal stability, flame retardancy and chemical stability. The multiple vinyl functional groups contained in the compound will undergo thermal decomposition reaction at high temperature to form an expanded carbon layer, which can cover the surface of the material and form a protective layer that is difficult to burn and oxygen-isolated, preventing oxygen and fuel from contacting, thereby inhibiting the spread of flames. Therefore, octavinyl POSS can be used as a synergistic flame retardant to improve the mechanical properties, flame retardancy and compatibility of the material. Moreover, octavinyl POSS molecules can also self-assemble into vesicle structures of different sizes and shapes through intermolecular interactions according to different conditions and ratios. This structure can absorb and disperse energy under stress loading, play a buffering role, reduce the risk of stress concentration, and thus improve the toughness of the material; it can also combine with molecules such as proteins and lipids on the surface of molds, destroy their cell membrane structures, and inhibit their growth and reproduction.
[0023] Urushiol has antibacterial, antifouling, and heat-insulating properties, and is highly compatible with the substrate. Urushiol can penetrate into the mold cell membrane and combine with molecules such as proteins and lipids in the membrane, causing changes in the membrane structure, making it impossible for substances inside the mold cell to be transported and metabolized normally, and ultimately leading to cell death. In addition, urushiol can also inhibit the enzyme activity and DNA synthesis of mold, thereby inhibiting its growth and reproduction.
[0024] Octave vinyl POSS is modified by polyphenols, so that the problem of poor compatibility between ocave vinyl POSS and soybean protein can be improved, the interface compatibility between ocave vinyl POSS and SPI is improved, and the antibacterial, mildew-proof and flame-retardant effects of the SPI adhesive are improved; and the phenolic hydroxyl group in POSS-U is oxidized to quinone, which reacts with the amino group in SPI to generate a strong covalent bond, further enhancing the adhesive force of the adhesive and improving the water-resistant bonding strength; and the polyphenols can also promote the formation of ocave vinyl POSS molecular vesicle structures, so as to improve the toughness of the adhesive material.
[0025] In addition, borax is added to further promote the cross-linking between SPI and POSS-U, so that on the basis of the mutual force between SPI and POSS-U, a dense cross-linking network is formed under the action of borax, and SPI is fixed in the vesicle structure, thereby ensuring the structural stability of the adhesive.
[0026] Therefore, the present invention utilizes polyphenol to modify octavinyl POSS and cooperates with borax cross-linking to prepare a high-performance, mildew-proof and flame-retardant bio-based adhesive, thereby improving the performance of the plant protein-based wood adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 These are cross-sectional SEM images of different adhesive samples.
[0028] Figure 2 These are the mildew test pictures of different adhesive samples.
[0029] Figure 3 This is a graph showing the flame retardant performance test results of different adhesive samples. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0031] The preparation method of polyphenol-modified vinyl POSS-modified soybean protein adhesive comprises the following steps:
[0032] S1. Extraction of urushiol:
[0033] a. Mix raw lacquer and ethanol in a ratio of 1 g: 25-35 mL (preferably 1 g: 30 mL), and stir until the raw lacquer is evenly dispersed in the ethanol to obtain a raw lacquer ethanol solution;
[0034] b. Filter the raw lacquer ethanol solution several times to obtain a clear lacquer phenol solution;
[0035] c. Rotary evaporate the urushiol solution at 45-55°C and 100-150 rpm to remove ethanol to obtain a brown viscous liquid, which is urushiol (U).
[0036] S2. Preparation of POSS-U:
[0037] Urushiol and octavinyl POSS are mixed in a mass ratio of 2-5:1-3, and then 0.5-1.5% by mass of ammonium persulfate is added and mixed evenly to obtain POSS-U.
[0038] S3. Preparation of adhesive:
[0039] Sodium dodecyl sulfate is dissolved in water at a mass ratio of 5 to 10:800 to 1000, and 18% by mass of sodium hydroxide is added to adjust the pH to between 8 and 9, and then POSS-U, soy protein isolate and borax (SB) are added at a mass ratio of 3:12:0.5 to 3, and stirred at 400 to 450 rpm for 20 to 30 minutes with a magnetic stirrer, and stirred evenly to obtain a polyphenol-modified vinyl POSS modified soy protein adhesive. The protein content of the soy protein isolate is not less than 95%.
[0040] Embodiment 1:
[0041] The preparation method of polyphenol-modified vinyl POSS-modified soybean protein adhesive comprises the following steps:
[0042] S1. Extraction of urushiol:
[0043] a. Add 66.67g of raw lacquer and 2000mL of anhydrous ethanol into a beaker, and stir with a magnetic stirrer at room temperature until the raw lacquer is evenly dispersed in the anhydrous ethanol to obtain a raw lacquer ethanol solution; the AR of the anhydrous ethanol is ≥99.7%;
[0044] b. Pour the raw lacquer ethanol solution into a Buchner funnel for suction filtration in several times, pad two layers of filter paper each time, repeat twice to obtain a clear lacquer phenol solution;
[0045] c. Evaporate the urushiol solution at 45-55°C and 100-150 rpm using a rotary evaporator to remove ethanol to obtain a brown viscous liquid, which is urushiol (U).
[0046] S2. Preparation of POSS-U:
[0047] d. Use a dropper to take 9 g of urushiol into a beaker, add 6 g of octavinyl POSS into the beaker, and mix well with a magnetic stirrer to obtain a mixture A;
[0048] e. Add 0.15 g of ammonium persulfate (APS) to mixture A, and then stir with a magnetic stirrer at room temperature for 5 to 10 minutes to mix evenly to obtain POSS-U.
[0049] S3. Preparation of adhesive:
[0050] 88 g of deionized water and 0.7 g of sodium dodecyl sulfate were mixed, 18% by mass of sodium hydroxide was added to adjust the pH to between 8 and 9, and then 3 g of POSS-U, 12 g of soy protein isolate and 0.5 g of borax (SB) were added, and the mixture was stirred at 400 to 450 rpm with a magnetic stirrer for 20 to 30 min to obtain a polyphenol-modified vinyl POSS modified soy protein adhesive, which was recorded as SPI / POSS-U / SB-0.5.
[0051] Embodiment 2:
[0052] This embodiment is substantially the same as embodiment 1, except that the mass of borax is 1.5 g, and the obtained adhesive is recorded as SPI / POSS-U / SB-1.5.
[0053] Embodiment 3:
[0054] This embodiment is substantially the same as embodiment 1, except that the mass of borax is 2.5 g, and the obtained adhesive is recorded as SPI / POSS-U / SB-2.5.
[0055] Comparative Example 1:
[0056] 12 g of soy protein isolate was added to 88 g of deionized water, and stirred with a magnetic stirrer at 400-450 rpm for 20-30 min to obtain a pure soy protein adhesive, which was denoted as SPI.
[0057] Appearance inspection:
[0058] The end surfaces of the adhesives prepared in Examples 1-3 and Comparative Example 1 were observed using a scanning electron microscope, and the obtained electron microscope images are as follows: Figure 1 shown.
[0059] Depend on Figure 1It can be seen that the cross-sectional SEM image of the pure soy protein adhesive of comparative example 1 shows a loose and porous structure, which is due to the weak intermolecular interaction force of SPI, which easily makes the adhesive brittle and has poor water resistance. After introducing POSS-U / SB, the fracture surface of embodiment 1 presents an initial vesicle structure, but still has less holes. When the borax addition amount is 1.5g, an orderly arranged vesicle structure is observed on the SEM image of embodiment 2. This is because the octaethylene POSS molecules self-assemble to form a vesicle structure under the assistance of polyphenols, which not only promotes the formation of the vesicle structure, but also increases the interface compatibility between octaethylene POSS and SPI. Interaction force is formed between SPI and POSS-U, and cross-linking occurs under the action of borax to form a dense cross-linked network, which fixes SPI in the vesicle structure. The cavity inside the vesicle structure can play a buffering role, absorb and disperse stress, reduce the risk of stress concentration, and thus improve the toughness of the soy protein adhesive. Along with the increase of SB content, embodiment 3 presents a ruptured and deformed vesicle, which is that the excessive borax does not carry out a cross-linking reaction. It can be seen that after adding 1.5g of borax, the cross-sectional morphology of the adhesive is optimal and the adhesive layer is most stable.
[0060] Performance Test:
[0061] 1. Dry / wet strength test: The adhesives prepared in Examples 1-3 and Comparative Example 1 were used to perform performance tests on indoor plywood samples according to the national standard GB / T17657-2013.
[0062] The test method is as follows: ① Select a poplar veneer with a size of 20cm*20cm*0.15cm and a moisture content of 10%. The coating density (each surface) is 180g / m 2 1. Apply adhesive to both sides of the core veneer, press the three-layer veneer in the direction perpendicular to the grain, and use hot pressing time (1.0MPa) = 6min, temperature = 120℃ for hot pressing; 2. Test the bonding strength of the plywood after cooling the three-layer plywood at room temperature for 24 hours, and saw the cooled plywood sample into a 25mm×100mm specimen; 3. Soak the specimen in hot water (63±3) for 3 hours, take it out and dry it at room temperature for 10min. Use a universal mechanical testing machine to test the dry / wet shear strength of the plywood, and set the loading rate to 10.0mm / min. The dry / wet strength test results of each embodiment and comparative example are shown in Table 1.
[0063] Table 1 Dry / wet shear strength of plywood
[0064] Serial number Example 1 Example 2 Example 3 Comparative Example 1 Dry strength(MPa) 1.48 2.46 1.58 1.23 Wet strength (MPa) 0.61 0.74 0.58 0.5
[0065] It can be seen from the data in Table 1 that with the addition of POSS-U / SB, the dry / wet shear strength of the adhesive first increases and then decreases. The addition of POSS-U enhances the cohesive strength of the adhesive because the phenolic hydroxyl groups in POSS-U are oxidized to quinones and react with the amino groups in SPI to produce strong covalent bonds, further enhancing the adhesion of the adhesive. SB further promotes the crosslinking between SPI and POSS-U.
[0066] The wet shear strength of the adhesive of Example 2 at 63°C water temperature is 0.74MPa, which meets the national standard of China Class I plywood (GB / T 17657-2013). When an excessive amount of SB is added, the wet shear strength of the adhesive decreases because SB is hydrophilic and can attract water molecules. The dry shear strength of the plywood prepared by the adhesive follows a trend similar to the wet shear strength. The dry shear strength of the adhesive of Example 2 is 100% higher than that of Comparative Example 1, reaching 2.46MPa.
[0067] 2. Antifungal test: Antifungal directly affects the adhesion performance and durability of the resulting plywood. The adhesives prepared in Examples 1-3 and Comparative Example 1 were tested for antifungal properties within 0-144 hours. The test results are shown in Figure 2 In the figure, 0 represents the adhesive of comparative example 1, and 1 and 3 represent the adhesives of embodiments 1-3 respectively.
[0068] from Figure 2 It can be seen that pure soy protein adhesive is prone to mold growth due to its biological characteristics. It started to grow mold after 48 hours. As time went by, the mold gradually increased and produced a foul odor. In contrast, POSS-U / SB modified SPI adhesive did not grow mold within 0-144 hours, which is due to the antibacterial properties of phenolic substances in urushiol.
[0069] Urushiol can penetrate into the mold cell membrane and combine with proteins and lipids in the membrane, causing changes in the membrane structure, making it impossible for substances inside the mold cells to be transported and metabolized normally, and ultimately leading to cell death. In addition, urushiol can also inhibit the enzyme activity and DNA synthesis of molds, thereby inhibiting their growth and reproduction. POSS molecules have a smaller size and higher surface energy, and can combine with proteins and lipids on the surface of molds, destroying their cell membrane structure and inhibiting their growth and reproduction. Therefore, POSS-U modified soy protein adhesive has good mildew resistance.
[0070] 3. Flame retardant performance test: Use cone calorimeter to evaluate the flame retardant performance of different adhesives. Figure 3 As shown in a, the peak heat release rate (PHRR) of SPI adhesive is 283.1kW / m 2After adding POSS-U / SB, the heat release rate decreased, and the peak heat release rate of SPI / POSS-U / SB-2.5 adhesive decreased by 25.4% to 211.3kW / m 2 .Depend on Figure 3 b and 3c, it can be seen that the total heat release (THR) and total smoke release (TSR) curves of the POSS-U / SB adhesive are lower than those of the SPI adhesive. Figure 3 The fire performance index of SPI adhesive in d is 0.04m 2 s / kW, while the fire performance index of SPI / POSS-U / SB-2.5 adhesive is 0.07m 2 s / kW, which is 75% higher than that of SPI adhesive. All of the above indicate that the adhesive has better flame retardant properties after adding POSS-U / SB.
[0071] The reason is that the silicon-oxygen clusters (SiO 1.5 ) has high thermal stability and flame retardant properties, which can effectively prevent the spread of flames. Secondly, octavinyl POSS contains multiple vinyl functional groups, which will undergo thermal decomposition reactions at high temperatures to form an expanded carbon layer. The expanded carbon layer can cover the surface of the material, forming a protective layer that is difficult to burn and oxygen-isolated, preventing oxygen and fuel from contacting, thereby inhibiting the spread of flames.
Claims
1. The preparation method of polyphenol-modified vinyl POSS modified soybean protein adhesive is characterized in that: The following steps are involved: S1. Extraction of urushiol: a. Mixing raw lacquer and ethanol, and stirring until the raw lacquer is evenly dispersed in the ethanol to obtain a raw lacquer ethanol solution; b. Filter the raw lacquer ethanol solution to obtain a clear lacquer phenol solution; c. Rotary evaporation of the urushiol solution to remove ethanol to obtain a brown viscous liquid, which is urushiol; S2, uniformly mixing urushiol, octavinyl POSS and ammonium persulfate to obtain POSS-U; S3. Dissolve sodium dodecyl sulfate in water and adjust the pH to between 8 and 9. Then add POSS-U, soy protein isolate and borax and stir evenly to obtain a polyphenol-modified vinyl POSS modified soy protein adhesive.
2. the preparation method of the vinyl POSS modified soybean protein adhesive modified by polyphenols according to claim 1, is characterized in that: In step a of step S1, the usage ratio of raw lacquer and ethanol is 1 g: 25-35 mL.
3. The preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive according to claim 1, wherein: In step c of step S1, the rotary evaporation temperature is 45-55° C., and the rotary evaporation speed is 100-150 rpm.
4. the preparation method of the vinyl POSS modified soybean protein adhesive modified by polyphenols according to claim 1, is characterized in that: In step S2, the mass ratio of urushiol to octavinyl POSS is 2-5:1-3, and the mass percentage of ammonium persulfate is 0.5-1.5%.
5. the preparation method of the vinyl POSS modified soybean protein adhesive modified by polyphenols according to claim 4, is characterized in that: In step S2, the mass ratio of urushiol to octavinyl POSS is 3:2, and the mass of ammonium persulfate added is 1% of the total mass of urushiol and octavinyl POSS.
6. The preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive according to claim 1, wherein: In step S3, the mass ratio of sodium dodecyl sulfate to water is 5-10:800-1000.
7. The preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive according to claim 1, characterized in that: In step S3, the pH is adjusted by adding sodium hydroxide.
8. The preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive according to claim 1, wherein: In step S3, the mass ratio of POSS-U, SPI and borax is 3:12:0.5-3.
9. The preparation method of the polyphenol-modified vinyl POSS modified soybean protein adhesive according to claim 8, wherein: In step S3, the mass ratio of POSS-U, SPI and borax is 3:12:1.