Trivalent europium ion doped red fluorescent powder as well as preparation method and application thereof

Through the trivalent europium ion doped red phosphor Ca10Ag1-x(VO4)7:xEu3+, the problems of insufficient red light composition and low luminous efficiency in existing LEDs are solved, and high-efficiency red under near-ultraviolet and blue light excitation are achieved Light emission and chemical stability, suitable for white light illumination LEDs.

CN118995214APending Publication Date: 2024-11-22HUAIBEI NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088788.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When existing LED solutions excite yellow phosphors on blue LED chips to obtain white light, they lack red light components, resulting in low color index, and commercial red phosphors have low luminous efficiency and unstable chemical properties, making them difficult to be near-ultraviolet or Blue light excitation.

Method used

Provide a trivalent europium ion-doped red phosphor Ca10Ag1-x(VO4)7:xEu3+, which can emit red light under near-ultraviolet and blue light excitation, with good chemical stability, and mix calcium and silver sources. , vanadium and europium sources were prepared by calcination.

Benefits of technology

It realizes efficient red light emission under near-ultraviolet and blue light excitation, improves the color index and chemical stability of the LED, can match with near-ultraviolet and blue light LEDs, is suitable for white light illumination LEDs, and the use of Eu is low, saving raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995214A_ABST
    Figure CN118995214A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic luminescence, in particular to trivalent europium ion doped red fluorescent powder as well as a preparation method and application thereof. The chemical composition formula of the trivalent europium ion doped red fluorescent powder is Ca10Ag1-x (VO4) 7: xEu < 3 + >, wherein 0 < = x < = 1. The red fluorescent powder provided by the invention has good chemical stability, can obtain red light at about 618nm under the excitation of near ultraviolet (395nm) and blue light (466nm), can be matched with near ultraviolet and blue light LEDs, and is novel red fluorescent powder for white light LEDs. The Eu replaces the Ag position, and the Ag occupies few sites in the crystal of the compound, so that the mass of the used Eu is low while high doping can be realized, and raw materials are saved. The melting point of vanadium pentoxide is 923K, and in the preparation method, the reaction is in a molten state, so that the diffusion of atoms and the formation of a new phase are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic luminescence, and in particular to a red phosphor doped with trivalent europium ions and a preparation method and application thereof. Background Art

[0002] Photoluminescence refers to the phenomenon of luminescence produced by stimulating luminescent materials with ultraviolet, visible and infrared light. As the most promising new generation of solid-state light sources, light-emitting diodes (LEDs) play a very important role in lighting, bio-imaging, display and other fields closely related to national economic life due to their long service life, energy-saving and high efficiency, and green environmental protection.

[0003] Among all vanadate materials, YVO4 synthesized by Goldschmidt and Haraldscen in 1928 was discovered the earliest. YVO4 was then used in luminescent materials. In 1964, Eu was doped into YVO4. 3+ Ions successfully prepared YVO4:Eu that can emit red light 3+ Materials. 3+ After entering the lattice, it can replace the Y at the asymmetric center of the YO8 dodecahedron 3+ ions, thus promoting 5 D0→ 7 The transition intensity of F2 increases the intensity of the red light emitted. Compared with other red phosphors, it has obvious advantages in color and brightness and is widely used in the fields of lighting and display. Since then, vanadates have been studied in depth as phosphors, and people have a deeper understanding of their optical properties and energy transfer. The preparation methods are also increasing, making it a hot topic in phosphor research.

[0004] At present, the most mature commercial LED solution is to excite yellow phosphor on the blue LED chip to obtain white light. The typical method is to coat yttrium aluminum garnet (YAG: Ce) on the indium gallium nitride (InGaN) chip. 3+ ) phosphor. This method has low production cost and has been widely used. However, due to the lack of red light components, its color index is low and the color temperature is high, which limits the further application of LED. In addition, compared with other colors of phosphors, commercial red phosphors have lower luminous efficiency and are not chemically stable. Therefore, it is of great significance to find red phosphors that can be excited by near-ultraviolet or blue light and have excellent luminous performance.

[0005] At present, the market still lacks high-performance three-primary color phosphors for white light lighting LEDs based on near-ultraviolet or blue light diodes, especially red phosphors that can be excited by ultraviolet and blue light. Summary of the invention

[0006] Based on the above content, the present invention provides a trivalent europium ion doped red phosphor and its preparation method and application. The present invention solves the problem of low color rendering index due to low red light component in the emission spectrum in the prior art, and has good chemical stability and can be excited by near ultraviolet and blue light at the same time.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] One of the technical solutions of the present invention is a red phosphor doped with trivalent europium ions (hereinafter referred to as phosphor), the chemical composition formula of which is Ca 10 Ag 1-x (VO4)7:xEu 3+ ; where 0≤x≤1.

[0009] In some embodiments of the invention, 0.04≤x≤0.28.

[0010] A second technical solution of the present invention is a method for preparing the above-mentioned trivalent europium ion-doped red phosphor, comprising the following steps:

[0011] According to the chemical formula Ca 10 Ag 1-x (VO4)7:xEu 3+ The calcium source, the silver source, the vanadium source and the europium source are mixed and ground in a stoichiometric ratio to obtain a mixed material;

[0012] The mixed material is calcined to obtain the trivalent europium ion-doped red phosphor.

[0013] The third technical solution of the present invention is the use of the above-mentioned trivalent europium ion-doped red phosphor in the preparation of LEDs light-emitting devices.

[0014] A fourth technical solution of the present invention is a white light LED, comprising the above-mentioned red phosphor doped with trivalent europium ions.

[0015] The present invention discloses the following technical effects:

[0016] (1) The red phosphor of the present invention has good chemical stability and can obtain red light emission at about 618 nm under the excitation of near-ultraviolet (395 nm) and blue light (466 nm). It can match near-ultraviolet and blue light LEDs and is a new type of red phosphor for white light LEDs.

[0017] (2) Since Eu replaces the position of Ag, Ag occupies fewer lattice sites in the crystal of the compound, high doping can be achieved while the quality of Eu used is low, saving raw materials.

[0018] (3) The melting point of vanadium pentoxide is 923K. In the preparation method of the present invention, it is in a molten state during the reaction, which is conducive to the diffusion of atoms and the formation of new phases. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 The XRD spectrum of the phosphor prepared in Example 1-8; in the figure, CAVO: 0.04Eu 3+ Example 1, CAVO: 0.08Eu 3+ Example 2, CAVO: 0.12Eu 3+ Example 3, CAVO: 0.16Eu 3+ Example 4, CAVO: 0.20Eu 3+ Example 5, CAVO: 0.24Eu 3+ Example 6, CAVO: 0.28Eu 3+ represents Example 7, and CAVO represents Example 8.

[0021] Figure 2 This is the fluorescence emission spectrum of the phosphor prepared in Example 2 at 618 nm.

[0022] Figure 3 The fluorescence emission spectra of the phosphors prepared in Examples 1-7 at 395 nm; in the figure, 0.04 represents Example 1, 0.08 represents Example 2, 0.12 represents Example 3, 0.16 represents Example 4, 0.20 represents Example 5, 0.24 represents Example 6, and 0.28 represents Example 7.

[0023] Figure 4 The fluorescence emission spectra of the phosphors prepared in Examples 1-7 at 466 nm; in the figure, 0.04 represents Example 1, 0.08 represents Example 2, 0.12 represents Example 3, 0.16 represents Example 4, 0.20 represents Example 5, 0.24 represents Example 6, and 0.28 represents Example 7.

[0024] Figure 5 The CIE coordinate diagram (395nm excitation) of the phosphor prepared in Examples 1-7.

[0025] Figure 6The CIE coordinate diagram (466nm excitation) of the phosphor prepared in Examples 1-7. DETAILED DESCRIPTION

[0026] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0027] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0028] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0029] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0030] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0031] The first aspect of the present invention provides a trivalent europium ion doped red phosphor (referred to as phosphor) having a chemical composition formula of Ca 10 Ag 1-x (VO4)7:xEu 3+ ; where 0≤x≤1.

[0032] Eu replaces the position of Ag, and x is the activated ion Eu 3+ The molar percentage of the substituted metal ion Ag.

[0033] In some embodiments of the invention, 0.04≤x≤0.28.

[0034] In some embodiments of the present invention, the chemical formula is Ca 10 Ag 0.76 (VO4)7:0.24Eu 3+ .

[0035] A second aspect of the present invention provides a method for preparing the above-mentioned trivalent europium ion-doped red phosphor, comprising the following steps:

[0036] According to the chemical formula Ca 10 Ag 1-x (VO4)7:xEu 3+ The calcium source, the silver source, the vanadium source and the europium source are mixed and ground in a stoichiometric ratio to obtain a mixed material;

[0037] The mixed material is calcined to obtain the trivalent europium ion-doped red phosphor.

[0038] In some embodiments of the present invention, the calcium source is calcium carbonate; and the silver source is silver nitrate.

[0039] In some embodiments of the present invention, the vanadium source is vanadium pentoxide.

[0040] In some embodiments of the present invention, the europium source is europium oxide.

[0041] In some embodiments of the present invention, the calcination temperature is 800° C. to 1000° C., and the calcination time is 4 to 36 hours.

[0042] More preferably, the calcination temperature is 1000°C.

[0043] More preferably, the calcination time is 12 to 24 hours.

[0044] A third aspect of the present invention provides a use of the above-mentioned trivalent europium ion-doped red phosphor in the preparation of LEDs light-emitting devices.

[0045] A fourth aspect of the present invention provides a white light LED, comprising the above-mentioned red phosphor doped with trivalent europium ions.

[0046] The present invention is further described below by way of examples.

[0047] Example 1

[0048] According to the chemical composition formula of phosphor Ca 10 Ag 1-x (VO4)7:xEu 3+The raw materials were weighed in a stoichiometric ratio: europium oxide (Eu2O3) 0.0070 g, calcium carbonate (CaCO3) 1.009 g, silver nitrate (AgNO3) 0.1631 g, and vanadium pentoxide (V2O5) 0.6365 g.

[0049] The weighed europium oxide, calcium carbonate, silver nitrate and vanadium pentoxide are fully ground and mixed. Specifically, they are placed in a zirconium dioxide ball mill, and ball milled in a planetary ball mill at 500 rpm for 2 hours to obtain a mixed raw material; the mixed raw material is placed in a crucible and then sent to a muffle furnace for roasting, roasted at 1000°C for 24 hours, and naturally cooled to room temperature to obtain the first product. The first product is taken out and ground to obtain a phosphor. The composition of the obtained phosphor material is: Ca 10 Ag 0.96 Eu 0.04 (VO4)7.

[0050] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.3945, 0.242); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.574, 0.4085).

[0051] Example 2

[0052] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.92 Eu 0.08 (VO4)7, weigh 0.0141g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1563g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0053] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.448, 0.2647); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.6011, 0.3875).

[0054] Example 3

[0055] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.88 Eu 0.12 (VO4)7, weigh 0.0211g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1495g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0056] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.4558, 0.2651); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.6025, 0.3862).

[0057] Example 4

[0058] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.84 Eu 0.16 (VO4)7, weigh 0.0282g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1427g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0059] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.484, 0.2941); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.611, 0.3801).

[0060] Example 5

[0061] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.80 Eu 0.20 (VO4)7, weigh 0.0352g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1359g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0062] like Figure 3 As shown, the phosphor material of this embodiment emits a strong blue-green red light emission peak (600-640nm) under the excitation of 395nm ultraviolet light; Figure 4 It shows that its color coordinates are (0.5004, 0.2823); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.6178, 0.3741).

[0063] Example 6

[0064] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.76 Eu 0.24 (VO4)7, weigh 0.0422g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1291g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0065] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.5443, 0.3016); Figure 5 It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.6264, 0.3675).

[0066] Example 7

[0067] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag 0.72 Eu 0.28 (VO4)7, weigh 0.0493g of europium oxide (Eu2O3), 1.009g of calcium carbonate (CaCO3), 0.1223g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0068] like Figure 3 As shown, the phosphor prepared in this embodiment emits a strong blue-green red light emission peak (600-640nm) under 395nm ultraviolet light excitation; Figure 4 It shows that its color coordinates are (0.5538, 0.3192); Figure 5It showed that it emitted a strong red light emission peak (600-640nm) under 466nm visible light excitation; Figure 6 Its color coordinates are shown to be (0.5892, 0.3578).

[0069] It can be seen from the above content that the phosphors prepared in Examples 1 to 7 can be effectively excited by 395 nm near-ultraviolet and 466 nm blue light.

[0070] Figure 2 is the fluorescence emission spectrum of the phosphor prepared in Example 2 at 618 nm. Figure 2 It can be seen that this phosphor can be effectively excited by 395nm near-ultraviolet and 466nm blue light.

[0071] Figure 4 It is the fluorescence emission spectrum of the phosphor prepared in Example 1-7 at 466nm. Figure 4 This indicates that the doping concentration of trivalent europium ions can affect the final product, the phosphor Ca 10 Ag 1-x (VO4)7:xEu 3+ The luminous intensity of Eu 3+ As the concentration increases, the fluorescence intensity continues to increase. The fluorescence intensity is the highest when the doping concentration is 24% (x=0.24), and concentration quenching occurs when the doping concentration is 28% (x=0.28).

[0072] Example 8

[0073] The only difference from Example 1 is that the chemical composition formula of the phosphor is Ca 10 Ag(VO4)7, weigh 1.009g of calcium carbonate (CaCO3), 0.1700g of silver nitrate (AgNO3), and 0.6365g of vanadium pentoxide (V2O5).

[0074] Figure 1 The XRD spectrum of the phosphor prepared in Example 1-8; in the figure, CAVO: 0.04Eu 3+ Example 1, CAVO: 0.08Eu 3+ Example 2, CAVO: 0.12Eu 3+ Example 3, CAVO: 0.16Eu 3+ Example 4, CAVO: 0.20Eu 3+ Example 5, CAVO: 0.24Eu 3+ Example 6, CAVO: 0.28Eu 3+represents Example 7, and CAVO represents Example 8. The diffraction peak positions of the phosphors prepared in Examples 1 to 8 are consistent with the standard XRD card PDF#54-1149, indicating that the phosphor structures obtained in Examples 1 to 8 of the present invention are consistent with the matrix Ca 10 Ag(VO4)7, the product obtained in Example 8 is pure phase Ca 10 Ag(VO4)7, doping with trivalent europium ions does not change the Ca 10 Structure of Ag(VO4)7 matrix material.

[0075] The present invention not only provides a trivalent europium ion-doped red phosphor and a preparation method thereof, but also provides the use of the trivalent europium ion-doped red phosphor in the preparation of LEDs light-emitting devices, such as light-emitting diodes, three-primary-color fluorescent lamps or field emission displays.

[0076] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A red phosphor doped with trivalent europium ions, characterized in that: The chemical formula is Ca 10 Ag 1-x (VO4)7:xEu 3 + ; where 0≤x≤1.

2. The trivalent europium ion-doped red phosphor according to claim 1, characterized in that: 0.04≤x≤0.28。 3. The trivalent europium ion-doped red phosphor according to claim 1, characterized in that: The chemical formula is Ca 10 Ag 0.76 (VO4)7:0.24Eu 3+ .

4. A method for preparing a red phosphor doped with trivalent europium ions according to any one of claims 1 to 3, characterized in that: The following steps are involved: According to the chemical formula Ca 10 Ag 1-x (VO4)7:xEu 3+ The calcium source, the silver source, the vanadium source and the europium source are mixed and ground in a stoichiometric ratio to obtain a mixed material; The mixed material is calcined to obtain the trivalent europium ion-doped red phosphor.

5. The method for preparing a trivalent europium ion-doped red phosphor according to claim 4, characterized in that: The calcium source is calcium carbonate, calcium sulfate, calcium nitrate or anhydrous calcium chloride; the silver source is silver nitrate, silver sulfate or silver carbonate.

6. The method for preparing a trivalent europium ion-doped red phosphor according to claim 4, characterized in that: The vanadium source is vanadium pentoxide or ammonium vanadate.

7. The method for preparing a trivalent europium ion-doped red phosphor according to claim 4, characterized in that: The europium source is europium oxide.

8. The method for preparing a trivalent europium ion-doped red phosphor according to claim 4, characterized in that: The calcination temperature is 800° C. to 1000° C., and the calcination time is 4 to 36 hours.

9. Use of the trivalent europium ion-doped red phosphor according to any one of claims 1 to 3 in the preparation of LEDs.

10. A white light LED, characterized in that: The invention comprises the red phosphor doped with trivalent europium ions as claimed in any one of claims 1 to 3.