Composition for corrosive liquid and silicon oxide film thickness testing method
By using a composition of alkali and silicon oxide film protector in the corrosion solution, the bubble generation time is observed to measure the thickness of the silicon oxide film, which solves the problem of high measurement accuracy and cost in the prior art, and realizes the thickness of the silicon oxide film Fast and accurate monitoring.
Patent Information
- Application Number
- CN202411089928.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot accurately, quickly and at low cost to test the thickness of silicon oxide films, especially in semiconductor production lines. For silicon oxide films in key tunneling oxide cells, traditional methods such as optical thickness testing have low accuracy. Transmission electron microscope testing is costly and time-consuming, and cannot meet the needs of large-scale monitoring.
Provide a corrosion liquid containing alkali and silicon oxide film protector. The thickness of silicon oxide film is measured by observing the bubble generation time of silicon wafers in the corrosion liquid. The silane coupling agent, physical adsorbent, cationic surfactant and other groups are used. The adsorption effect of the fraction slows down the corrosion rate and ensures linear increase in corrosion time, thereby accurately measuring the film thickness.
It realizes accurate and rapid measurement of the thickness of silicon oxide film, reduces errors with traditional methods, is suitable for large-scale production line monitoring, is low in cost, and can effectively monitor the thickness changes of silicon oxide film.
Smart Images

Figure BDA0004986239350000121 
Figure BDA0004986239350000131 
Figure BDA0004986239350000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of film thickness testing and relates to a composition for etching liquid and a method for testing the thickness of a silicon oxide film. Background Art
[0002] At present, the thickness of silicon oxide films in semiconductor production lines needs to be monitored regularly to ensure the stability of the film growth process of the production line. If the growth process fluctuates, it will lead to too thin or too thick silicon oxide films, which will affect the device. More seriously, it will cause the device to malfunction and be scrapped. This is especially true for silicon oxide films that play a key role, such as the silicon oxide film that serves as the tunneling layer in the tunnel oxide layer battery (Topcon). The tunneling layer is generally formed by an ultra-thin silicon oxide film with a thickness of 1nm to 3nm. Therefore, it is necessary to perform precise thickness testing of the silicon oxide film and rapid testing of large quantities of silicon oxide films for regular monitoring.
[0003] At present, conventional optical thickness testers are mainly used to test the thickness of silicon oxide films. However, the accuracy of the measured thickness of silicon oxide films is low, and it can only be used for parallel comparison and cannot be used as a reference for the actual accurate thickness value. Transmission electron microscopy can accurately test the thickness of the tunneling layer, but the transmission electron microscopy test is very expensive and takes a long time to test. It is not suitable as a means of testing the thickness of silicon oxide films on large quantities of silicon wafers, and cannot be used to monitor the thickness of silicon oxide films on the production line.
[0004] Therefore, a more accurate, efficient and low-cost method is needed to test the thickness of silicon oxide films. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention provides a composition for etching liquid and a method for testing the thickness of silicon oxide film.
[0006] In order to achieve the above-mentioned purpose, as the first aspect of the present invention, a composition for etching liquid is provided, which comprises an alkali and a silicon oxide film protective agent, wherein the silicon oxide film protective agent comprises a silane coupling agent, a physical adsorbent with a long carbon chain, a cationic surfactant and a metal salt, and the physical adsorbent is used to be adsorbed on the surface of silicon.
[0007] Furthermore, the mass fraction of the silane coupling agent in the etching solution is between 0.05wt% and 0.5wt%, the mass fraction of the physical adsorbent in the etching solution is between 0.01wt% and 0.05wt%, the mass fraction of the cationic surfactant in the etching solution is between 0.01wt% and 0.05wt%, the mass fraction of the metal salt in the etching solution is between 0.2wt% and 1wt%, and the mass fraction of the alkali in the etching solution is between 0.2wt% and 1wt%.
[0008] Furthermore, the cationic surfactant includes a quaternary ammonium salt.
[0009] Furthermore, the physical adsorbent includes at least one of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium bromide, and the base includes sodium hydroxide and / or potassium hydroxide.
[0010] As a second aspect of the present invention, a method for testing the thickness of a silicon oxide film is disclosed, comprising:
[0011] Determining the etching rate of the silicon oxide film in an etching solution, wherein the solute of the etching solution includes the above-mentioned composition;
[0012] Placing a silicon wafer to be tested in the etching solution, wherein the silicon wafer to be tested comprises a silicon substrate and a silicon oxide film formed on the surface of the silicon substrate;
[0013] Recording the time when at least one bubble appears in the etching solution on the silicon wafer to be tested, and taking the time as the total etching time;
[0014] The thickness of the silicon oxide film is determined according to the total etching time and the etching rate.
[0015] Furthermore, placing the silicon wafer to be tested before the etching solution also includes:
[0016] At least one silicon wafer to be tested corresponding to at least one position is extracted from multiple batches of silicon wafers, wherein the multiple batches of silicon wafers are from the same furnace tube.
[0017] Further, determining the corrosion rate of the silicon oxide film in the etching solution includes:
[0018] Measuring the thickness of the silicon oxide film of the silicon wafer sample by using a transmission electron microscope, wherein the performance of the silicon oxide film on the surface of the silicon wafer sample is consistent with the performance of the silicon oxide film of the silicon wafer to be measured, and the size of the silicon wafer sample is smaller than the size of the silicon wafer to be measured;
[0019] placing the silicon wafer sample in the etching solution;
[0020] Recording the time when at least one bubble appears in the etching solution on the silicon wafer sample, and taking the time as the total etching time;
[0021] The etching rate is determined according to the total etching time and the thickness of the silicon oxide film.
[0022] Furthermore, the average thickness of the silicon oxide film satisfies the following formula:
[0023] D = (t1 + ... + tn) * v / n;
[0024] Wherein, D is the average thickness of the silicon oxide film;
[0025] t1 is the total corrosion time obtained when one bubble appears on the surface of the silicon wafer to be tested, and tn is the total corrosion time obtained when n bubbles appear on the surface of the silicon wafer to be tested, where n is greater than or equal to 2;
[0026] v is the corrosion rate.
[0027] Furthermore, the thickness of the silicon oxide film satisfies the following formula:
[0028] Dm=tm*v;
[0029] Wherein, Dm is the thickness of the silicon oxide film at (Xm, Ym);
[0030] (Xm, Ym) is the position where the mth bubble appears on the surface of the silicon wafer to be tested;
[0031] tm is the total corrosion time corresponding to the occurrence of the mth bubble on the surface of the silicon wafer to be tested;
[0032] v is the corrosion rate.
[0033] Furthermore, the silicon oxide film includes a tunneling silicon oxide film.
[0034] The beneficial effects of the present invention are:
[0035] The composition for etching liquid of the present invention comprises alkali, and alkali etching silicon oxide generates soluble silicate and water, and alkali etching silicon generates hydrogen. When a silicon wafer with a silicon oxide film on the surface is placed in the alkali etching liquid for etching, it can be judged whether the silicon oxide film is completely etched by observing whether bubbles are generated, and the amount of silicon oxide etched by the alkali etching liquid increases approximately linearly with the etching time. Under specific etching conditions, the etching rate is approximately constant, and the thickness of the silicon oxide film can be obtained by multiplying the etching time by the etching rate. The silicon oxide film protective agent is adsorbed on the silicon hydroxyl group on the surface of the silicon oxide film by chemical adsorption, physical adsorption and electrostatic adsorption, thereby slowing down the etching rate of the alkali on the silicon oxide film, prolonging the etching time, weakening the violent corrosion reaction, and further making the etching amount increase linearly with the etching time, so that the measurement result is more accurate.
[0036] The silicon oxide film thickness testing method of the present invention can accurately and completely measure the thickness of the silicon oxide film by converting the time and corresponding position of the observed bubble appearance into the thickness data of the silicon oxide film and the corresponding position information. Compared with the traditional optical method for measuring the thickness of the silicon oxide film, the error between the silicon oxide film thickness measured by the present invention and the actual silicon oxide film thickness is smaller. At the same time, the method of the present invention is convenient and fast, which is conducive to monitoring the thickness of the silicon oxide film on the production line and monitoring the thickness of the silicon oxide film of a large number of silicon wafers of the same batch.
[0037] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. In addition, there are multiple features, elements, and components that appear in each of the following texts and drawings, and different symbols or numbers are marked for convenience, but they all represent components with the same or similar structures or functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The present invention will be further described below in conjunction with the accompanying drawings:
[0039] Figure 1 A flow chart of an implementation method of the silicon oxide film thickness testing method provided by the present invention;
[0040] Figure 2 A flow chart of an implementation method of determining the etching rate of a silicon oxide film in an etching solution provided by the present invention. DETAILED DESCRIPTION
[0041] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.
[0042] References to "one embodiment" or "an example" or "an example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed in the present application. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.
[0043] As a first aspect of the present invention, a composition for etching liquid is provided, which comprises an alkali and a silicon oxide film protective agent, wherein the silicon oxide film protective agent comprises a silane coupling agent, a physical adsorbent having a long carbon chain, a cationic surfactant and a metal salt, and the physical adsorbent is used to be adsorbed on the surface of silicon.
[0044] The composition for etching liquid of the present invention comprises alkali, and alkali corrodes silicon oxide to generate soluble silicate and water, and alkali solution corrodes silicon oxide film to generate hydrogen. When a silicon wafer with silicon oxide film on the surface is placed in alkali etching liquid for etching, whether the silicon oxide is completely corroded can be judged by observing whether bubbles are generated, and the amount of silicon oxide corroded by the alkali etching liquid increases approximately linearly with the corrosion time. Under the set corrosion conditions, the corrosion rate is approximately constant, and the thickness of the silicon oxide film can be obtained by multiplying the corrosion time by the corrosion rate. The silicon oxide film protective agent acts on the silicon hydroxyl group on the surface of the silicon oxide film by chemical adsorption, physical adsorption and electrostatic adsorption, so that the silicon and hydroxyl group have stronger bonding force, thereby slowing down the corrosion rate of the alkali on the silicon oxide film, prolonging the corrosion time, weakening the violent corrosion reaction, and further making the corrosion amount increase linearly with the corrosion time, so that the measurement result is more accurate.
[0045] The hydrolyzed silanol groups of the silane coupling agent can condense with the hydroxyl groups on the surface of silicon dioxide and adsorb to the surface of silicon oxide through chemical bonds, thereby grafting long carbon chains on the surface of silicon oxide to hinder the corrosion of silicon oxide by alkali.
[0046] The present invention does not specifically limit the physical adsorbent with a long carbon chain. When the physical adsorbent with a long carbon chain is used as a surfactant, the surface tension of the solution is reduced, the wettability of the etching solution and the silicon wafer surface is improved, and the generated bubbles are promoted to separate from the silicon wafer. At the same time, the physical adsorbent with a long carbon chain is hydrolyzed in the etching solution to form a non-polar group with a long carbon chain, which can be physically adsorbed on the surface of the silicon wafer, and can prevent the silicon oxide film from reacting with the alkaline etching solution, thereby slowing down the corrosion rate. Preferably, the physical adsorbent with a long carbon chain is at least one of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium bromide.
[0047] The present invention does not specifically limit the cationic surfactant and the metal salt. The silicon oxide film has the characteristic of being negatively charged in an alkaline environment. When a cationic surfactant or a metal salt is added, the silicon oxide film generates an electrostatic effect with the metal cations generated by the hydrolysis of the cationic surfactant or the metal salt in an alkaline environment. The silicon oxide film will electrostatically adsorb the above-mentioned positively charged substances in an alkaline environment, forming protection on the surface of the silicon oxide film, which can prevent the silicon oxide film from reacting with the alkaline etching solution and slow down the corrosion rate. The cationic surfactant adopts a component that is easily soluble in an alkaline solution and does not react with other compositions, and preferably includes a quaternary ammonium salt. The quaternary ammonium salt has an adsorption effect on the silicon surface, which can prevent the alkali from corroding the silicon oxide, thereby slowing down the corrosion rate. The metal salt is preferably at least one of a chloride metal salt, a sulfate metal salt, a carbonate metal salt and a nitrate metal salt.
[0048] The oxide film protective agent of the present invention has multiple components, and the adsorption mechanisms of the multiple components are different. Those skilled in the art can reasonably adjust the proportions of the different components to further make the corresponding adsorption effect larger or smaller.
[0049] Preferably, the mass fraction of the silane coupling agent in the etching solution is between 0.05wt% and 0.5wt%, the mass fraction of sodium dodecylbenzene sulfonate in the etching solution is between 0.01wt% and 0.05wt%, the mass fraction of the cationic surfactant in the etching solution is between 0.01wt% and 0.05wt%, the mass fraction of the metal cation in the etching solution is between 0.2wt% and 1wt%, the alkali is sodium hydroxide with a mass fraction in the etching solution between 0.2wt% and 1wt%, and the remainder of the etching solution is deionized water.
[0050] In some embodiments, the base of the present invention comprises potassium hydroxide and / or sodium hydroxide.
[0051] Silicon oxide film protective agent avoids the problem that the corrosion time is too fast and the bubble recording time cannot be accurately observed to calculate the corresponding film thickness. By adding silicon oxide film protective agent, corrosion and protection occur at the same time, slowing down the corrosion rate and increasing the corrosion time, thereby achieving the effect of accurate measurement.
[0052] The corrosion rate of the silicon oxide film in the etching solution can be adjusted by adjusting the temperature, alkali concentration and the concentration of the silicon oxide film protective agent, so that the test data of the silicon oxide film thickness can be more accurate. Preferably, when the corrosion rate is less than or equal to 0.001nm / s, the test data of the silicon oxide film thickness of the present invention can have extremely high accuracy.
[0053] As a second aspect of the present invention, a method for testing the thickness of a silicon oxide film is disclosed, comprising:
[0054] In step S110, the etching rate of the silicon oxide film in the etching solution is determined;
[0055] In step S120, the silicon wafer to be tested is placed in the above-mentioned etching solution, and the silicon wafer to be tested includes a silicon substrate and a silicon oxide film formed on the surface of the silicon substrate;
[0056] In step S130, the time when at least one bubble appears in the etching solution on the silicon wafer to be tested is recorded, and the time is taken as the total etching time;
[0057] In step S140, the thickness of the silicon oxide film is determined according to the total etching time and the etching rate.
[0058] The silicon oxide film thickness testing method of the present invention can accurately measure the thickness of the silicon oxide film. Compared with the traditional optical method for measuring the thickness of the silicon oxide film, the error between the silicon oxide film thickness measured by the present invention and the actual silicon oxide film thickness is smaller. At the same time, the method is convenient and fast, which is conducive to monitoring the thickness of the silicon oxide film on the production line and monitoring the silicon oxide film thickness of a large number of silicon wafers of the same batch.
[0059] like Figure 2 As shown, determining the etching rate of the silicon oxide film in the above etching solution specifically includes the following steps:
[0060] In step S111, a transmission electron microscope is used to measure the thickness of a silicon oxide film on a silicon wafer sample;
[0061] In step S112, a silicon wafer sample is placed in the above-mentioned etching solution, the performance of the silicon oxide film on the surface of the silicon wafer sample is consistent with the performance of the silicon oxide film on the above-mentioned silicon wafer to be tested, and the size of the silicon wafer sample is smaller than the size of the above-mentioned silicon wafer to be tested;
[0062] In step S113, the time when at least one bubble appears in the etching solution on the silicon wafer sample is recorded, and the time is taken as the total etching time;
[0063] In step S114, the etching rate is determined according to the total etching time and the thickness of the silicon oxide film.
[0064] For ease of understanding, the following explains how to determine the etching rate of a silicon oxide film in an etching solution by means of an example.
[0065] First, the thickness of the silicon oxide film on the silicon wafer sample was measured using a transmission electron microscope, which was d;
[0066] The silicon wafer sample is placed in the etching solution, the performance of the silicon oxide film on the surface of the silicon wafer sample is consistent with the performance of the silicon oxide film on the silicon wafer to be tested. As an optional implementation method, the silicon oxide film on the surface of the silicon wafer sample and the silicon oxide film on the silicon wafer to be tested are grown by the same silicon oxide film growth method, and the process parameters for growing the silicon oxide film are also the same; the size of the silicon wafer sample is smaller than the size of the silicon wafer to be tested;
[0067] The time when at least one bubble appears on the silicon wafer sample is recorded as t;
[0068] From this we can see that the corrosion rate of silicon oxide film in the etching solution is d / t.
[0069] To ensure accurate measurement, the performance of the silicon oxide film on the surface of the silicon wafer sample is consistent with the performance of the silicon oxide film on the silicon wafer to be tested. Specifically, the silicon oxide films of the silicon wafer sample and the silicon wafer to be tested are formed by the same oxidation method. Optionally, the two silicon oxide films are formed by the same oxidation equipment, and the process parameters of the oxidation methods of the two silicon oxide films are also the same.
[0070] like Figure 1 As shown, in step S120, the silicon wafer to be tested is placed before the etching solution, and the step also includes: extracting at least one silicon wafer to be tested corresponding to at least one position from multiple batches of silicon wafers, wherein the multiple batches of silicon wafers come from the same furnace tube.
[0071] In some embodiments, the testing method of the present invention can be used to monitor the thickness of the silicon oxide tunneling layer on the surface of TOPcon silicon substrate solar cells in a production line. Specifically, silicon wafers grown with silicon oxide films from the same batch in the same furnace tube can be selected, and silicon wafers grown at different positions of the furnace tube can be selected for silicon oxide film thickness testing. The silicon oxide film thickness data of silicon wafers grown at multiple positions of the furnace tube can reflect the overall stability of the silicon oxide film grown in the furnace tube, and monitor and measure the thickness uniformity. Preferably, silicon wafers located at the upper, middle and lower positions of the furnace tube can be selected for silicon oxide film thickness testing.
[0072] In other embodiments, silicon wafers grown with silicon oxide films from different batches in the same furnace tube are selected, and any number of silicon wafers from different batches are selected to perform silicon oxide film thickness tests to obtain silicon oxide film thickness data from different batches to monitor the process stability of the furnace tube;
[0073] In step S120, the present invention does not specifically limit how to obtain the silicon wafer to be tested, and the silicon wafer to be tested can be obtained by external purchase. For another example, the silicon wafer can be obtained by preparing a silicon oxide film on the silicon wafer.
[0074] The present invention does not specifically limit the type of silicon wafer. It only needs to satisfy that there is a silicon oxide film on the silicon wafer. For example, it can be a silicon wafer used as a Topcon battery, and a tunneling oxide layer is grown on the silicon wafer. For another example, it can be a silicon wafer used as a field effect transistor, and a gate oxide is grown on the silicon wafer. For another example, it can be a monitoring silicon wafer for a furnace tube, and a silicon oxide film corresponding to the furnace tube is grown on the silicon wafer.
[0075] In step S130, the time when at least one bubble appears in the above-mentioned etching solution on the silicon wafer to be tested is recorded, and the time is used as the total etching time; the silicon oxide film thickness testing method of the present invention can accurately measure the thickness of the silicon oxide film by converting the time of observing the appearance of bubbles into the thickness data of the silicon oxide film, and it is convenient and fast.
[0076] In some embodiments, the position where the first bubble appears is converted to the position where the silicon oxide film is thinnest, and the corresponding corrosion time multiplied by the corrosion rate is the thickness of the silicon oxide film at the thinnest point. Compared with other thickness testing methods, it is difficult to find the thinnest film thickness. The method of the present invention accurately and quickly finds the thinnest film thickness and the corresponding thickness of the thinnest silicon oxide film; the position where the last bubble appears is converted to the position where the silicon oxide film is thickest, and the corresponding corrosion time multiplied by the corrosion rate is the thickness of the thickest silicon oxide film. The method of the present invention accurately and quickly finds the positions of the thinnest and thickest points of the silicon oxide film in the silicon wafer and the corresponding film thickness data, thereby judging the in-wafer uniformity of the silicon oxide film thickness.
[0077] In step S140, the thickness of the silicon oxide film is determined according to the total etching time and the etching rate. The thickness of the silicon oxide film is equal to the product of the total etching time and the etching rate.
[0078] The present invention does not specifically limit how to apply the silicon oxide film thickness testing method of the present invention.
[0079] In some embodiments, the average thickness of the silicon oxide film satisfies the following formula:
[0080] D = (t1 + ... + tn) * v / n;
[0081] Where D is the average thickness of the silicon oxide film;
[0082] t1 is the total corrosion time obtained when one bubble appears on the surface of the silicon wafer to be tested, and tn is the total corrosion time obtained when n bubbles appear on the surface of the silicon wafer to be tested, where n is greater than or equal to 2;
[0083] v is the corrosion rate.
[0084] In other embodiments, when multiple bubbles appear on the surface of the silicon wafer to be tested, the positions corresponding to the multiple bubbles and the corresponding multiple corrosion times are obtained, and the multiple corrosion times and corrosion rates are multiplied to obtain multiple silicon oxide film thicknesses, and the silicon oxide film thicknesses at multiple corresponding positions of the silicon wafer to be tested are obtained to obtain the silicon oxide film thickness distribution information of the silicon wafer to be tested.
[0085] For ease of understanding, the following explains how to obtain the silicon oxide film thickness distribution information by using an example.
[0086] First, place the silicon wafer to be tested in the above-mentioned etching solution, and use XY coordinates to describe the position where the bubbles appear on the silicon wafer to be tested;
[0087] The time when the first bubble appears on the silicon wafer to be tested is recorded as t1, and the corresponding bubble appearance position is (X1, Y1); the time when the second bubble appears on the silicon wafer to be tested is recorded as t2, and the corresponding bubble appearance position is (X1, Y1); ... the time when the mth bubble appears on the silicon wafer to be tested is recorded as tm, and the corresponding bubble appearance position is (Xm, Ym);
[0088] The etching rate of the silicon oxide film is v according to the set temperature, the set etching solution and the etching solution concentration, the set protective agent and the protective agent concentration;
[0089] It can be seen that the film thickness at the position (X1, Y1) is t1*v, the film thickness at the position (X2, Y2) is t2*v, ..., the film thickness at the position (Xm, Ym) is tm*v, and the XYZ coordinates are used to represent the thickness distribution information of the silicon oxide film on the silicon wafer to be tested, the Z coordinate represents the thickness of the silicon oxide film, and the X and Y coordinates represent the positions where bubbles appear on the silicon wafer to be tested. By drawing a graph based on the above data, the thickness distribution information of the silicon oxide film on the silicon wafer to be tested can be obtained.
[0090] By observing the positions and corresponding times of the bubbles appearing one after another, the regional distribution of the silicon oxide film thickness in the silicon wafer can be quickly determined and the thickness can be calculated, so that the silicon oxide film thickness distribution information can be quickly and accurately obtained.
[0091] The present invention does not specifically limit the type of silicon oxide film. The silicon oxide film may be a silicon oxide film grown by wet oxygen, a silicon oxide film grown by dry oxygen, or a silicon oxide film grown by plasma enhanced chemical vapor deposition.
[0092] The present invention does not impose any special limitation on the thickness of the silicon oxide film. In order to shorten the test time, preferably, the thickness of the silicon oxide film is within 30 nm. The etching solution prepared by the composition of the present invention and the test method can quickly and accurately obtain the test thickness of the silicon oxide film.
[0093] The present invention will be further explained below in conjunction with the embodiments.
[0094] Preparation Example
[0095] Preparation Example 1
[0096] Prepare a corrosive solution, including:
[0097] Weigh 0.2 g of a silicon coupling agent, 0.04 g of sodium dodecylbenzenesulfonate, 0.04 g of dodecyltrimethylammonium bromide, 0.5 g of magnesium chloride, and 2 g of sodium hydroxide to obtain a composition;
[0098] Add 97.22 g of deionized water to the composition to obtain etching solution 1;
[0099] The etching solution 2 has the same components as the etching solution 1, except that the mass of sodium hydroxide in the etching solution 2 is 1 g; the etching solution 3 has the same components as the etching solution 1, except that the mass of sodium hydroxide in the etching solution 3 is 0.5 g;
[0100] The components and contents of the etching solution are shown in Table 1 below.
[0101] Table 1
[0102]
[0103] Preparation Example 2
[0104] Prepare a corrosive solution, including:
[0105] Weigh 0.2 g of a silicon coupling agent, 0.04 g of sodium dodecylbenzenesulfonate, 0.04 g of dodecyltrimethylammonium bromide, 0.5 g of magnesium chloride, and 0.5 g of sodium hydroxide to obtain a composition;
[0106] 98.92 g of deionized water was added to the composition to obtain etching solution 4;
[0107] The etching solution 5 has the same components as the etching solution 4, except that the etching solution 5 contains 0.2 g of silane coupling agent, 0.05 g of sodium dodecylbenzenesulfonate, and 0.05 g of dodecyltrimethylammonium bromide. The etching solution 6 has the same components as the etching solution 4, except that the etching solution 6 contains 0.5 g of silane coupling agent, 0.05 g of sodium dodecylbenzenesulfonate, 0.05 g of dodecyltrimethylammonium bromide, and 0.7 g of magnesium chloride.
[0108] The components and contents of the etching solution are shown in Table 2 below.
[0109] Table 2
[0110]
[0111] Example
[0112] Example 1
[0113] Determining the corrosion rate of the silicon oxide film in the etching solution specifically includes the following steps:
[0114] Step 1: Use transmission electron microscopy to test the thickness of the silicon oxide film on the silicon wafer sample to be 1.8nm;
[0115] Step 2: placing three silicon wafer samples in the three etching solutions in Preparation Example 1, with the temperature of the etching solution being 50° C.
[0116] Step 3: Record the time from the beginning to the appearance of bubbles on the three silicon wafer samples in the three etching solutions, and use this time as the total etching time. The etching solutions and corresponding etching times are recorded in Table 3;
[0117] Step 4: Determine the corrosion rate based on the total corrosion time and the thickness of the silicon oxide film. The corrosion rate is the ratio of the silicon oxide film thickness tested in the first step to the total corrosion time in the third step. The corrosion rate is shown in Table 3.
[0118] Table 3
[0119]
[0120] The present invention reduces the concentration of alkali components in the etching solution and prolongs the etching time, thereby reducing the etching rate, and further makes the etching amount increase linearly with the etching time, so that the measurement result is more accurate. The sodium hydroxide concentration of the etching solution 3 is the lowest, and the etching rate of the silicon oxide film is the smallest, reaching 0.00295nm / s. Selecting the etching solution 3 as the etching solution for testing the thickness of the silicon oxide film can obtain a more accurate thickness.
[0121] A thermal oxidation method is used to set a process procedure for growing a 1.8 nm silicon oxide film. The silicon wafer to be tested, on which a silicon oxide film is grown by the above method, is placed in the etching solution 3 to start etching. The temperature of the etching solution is 50°C until bubbles appear on the surface of the silicon wafer to be tested and the etching stops. The etching time is recorded as 10 minutes and 3 seconds. When recording the etching time when bubbles appear when the silicon wafer to be tested is placed in the etching solution, etching can be performed and recorded in a transparent container (containing glass-lined PFA). The container is filled with etching solution and placed in a constant temperature area, and a side camera is used to capture the surface state of the silicon wafer.
[0122] The above-mentioned etching time is multiplied by the etching rate of the etching solution 3 on the silicon oxide film determined above, which is 0.00295nm / s, to obtain the silicon oxide film thickness of 1.779nm, which is basically consistent with the data of growing a 1.8nm silicon oxide film set by the thermal oxidation method. The etching solution and silicon oxide film thickness testing method of the present invention can obtain accurate silicon oxide film thickness.
[0123] Example 2
[0124] Determining the corrosion rate of the silicon oxide film in the etching solution specifically includes the following steps:
[0125] Step 1: Use transmission electron microscopy to test the thickness of the silicon oxide film on a standard silicon wafer to be 1.8nm;
[0126] Step 2: placing three silicon wafer samples in the three etching solutions in Preparation Example 2, with the temperature of the etching solution being 50° C.
[0127] Step 3: Record the time from the beginning to the appearance of bubbles for the three silicon wafer samples in the three etching solutions, and use this time as the total etching time. The etching solutions and corresponding etching times are recorded in Table 4.
[0128] Step 4: Determine the corrosion rate based on the total corrosion time and the thickness of the silicon oxide film. The corrosion rate is the ratio of the silicon oxide film thickness tested in the first step to the total corrosion time in the third step. The corrosion rate is shown in Table 4.
[0129] Table 4
[0130]
[0131] The present invention increases the component concentration of the silicon oxide film protective agent in the etching solution and prolongs the etching time, thereby reducing the etching rate, further making the etching amount increase linearly with the etching time, so that the measurement result is more accurate. The etching solution 6 increases the concentration of the silane coupling agent and the concentration of magnesium chloride. Therefore, the silicon oxide film protective agent in the etching solution 6 has stronger chemical adsorption and electrostatic adsorption effects. More protective agents are adsorbed on the surface of the silicon wafer to prevent the etching solution from corroding the surface. Therefore, the etching rate of the silicon oxide film by the etching solution 6 is minimized, reaching 0.00175nm / s. Selecting the etching solution 6 as the etching solution for testing the thickness of the silicon oxide film can obtain a more accurate thickness.
[0132] A thermal oxidation method is used to set a process procedure for growing a 1.5 nm silicon oxide film. The silicon wafer to be tested, on which the silicon oxide film is grown by the above method, is placed in an etching solution 6 and etching begins. The temperature of the etching solution is 50°C until bubbles appear on the surface of the silicon wafer to be tested and the etching stops. The etching time is recorded as 14 minutes and 25 seconds. The etching time is multiplied by the etching rate of the etching solution 6 on the silicon oxide film determined above, which is 0.00175 nm / s, to obtain a silicon oxide film thickness of 1.513 nm, which is basically consistent with the data set for growing a 1.5 nm silicon oxide film by the thermal oxidation method. The etching solution and silicon oxide film thickness testing method of the present invention can obtain accurate silicon oxide film thickness.
[0133] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.
Claims
1. A composition for a corrosive liquid, It is characterized in that The composition comprises: alkali and silicon oxide film protective agent, wherein the silicon oxide film protective agent comprises a silane coupling agent, a physical adsorbent with a long carbon chain, a cationic surfactant and a metal salt, and the physical adsorbent is used for being adsorbed on the surface of silicon.
2. The composition according to claim 1, It is characterized in that The mass fraction of the silane coupling agent in the etching solution is between 0.05% and 0.5%, the mass fraction of the physical adsorbent in the etching solution is between 0.01% and 0.05%, the mass fraction of the cationic surfactant in the etching solution is between 0.01% and 0.05%, the mass fraction of the metal salt in the etching solution is between 0.2% and 1%, and the mass fraction of the alkali in the etching solution is between 0.2% and 1%.
3. The composition according to claim 1, It is characterized in that The cationic surfactant includes a quaternary ammonium salt.
4. A composition according to any one of claims 1 to 3, It is characterized in that The physical adsorbent includes at least one of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium bromide, and the base includes sodium hydroxide and / or potassium hydroxide.
5. A method for testing the thickness of silicon oxide films. It is characterized in that include: Determining the corrosion rate of a silicon oxide film in an etching solution, wherein the solute of the etching solution comprises the composition according to any one of claims 1 to 4; Placing a silicon wafer to be tested in the etching solution, wherein the silicon wafer to be tested comprises a silicon substrate and a silicon oxide film formed on the surface of the silicon substrate; Recording the time when at least one bubble appears in the etching solution on the silicon wafer to be tested, and taking the time as the total etching time; The thickness of the silicon oxide film is determined based on the total etching time and the etching rate.
6. The method for testing the thickness of a silicon oxide film according to claim 5, It is characterized in that Placing the silicon wafer to be tested before the etching solution, further comprising: At least one silicon wafer to be tested corresponding to at least one position is extracted from multiple batches of silicon wafers, wherein the multiple batches of silicon wafers are from the same furnace tube.
7. The method for testing the thickness of a silicon oxide film according to claim 5, It is characterized in that Determining the corrosion rate of silicon oxide film in the etching solution includes: Measuring the thickness of the silicon oxide film of the silicon wafer sample by using a transmission electron microscope, wherein the performance of the silicon oxide film on the surface of the silicon wafer sample is consistent with the performance of the silicon oxide film of the silicon wafer to be measured, and the size of the silicon wafer sample is smaller than the size of the silicon wafer to be measured; placing the silicon wafer sample in the etching solution; Recording the time when at least one bubble appears in the etching solution on the silicon wafer sample, and taking the time as the total etching time; The etching rate is determined according to the total etching time and the thickness of the silicon oxide film.
8. The method for testing the thickness of a silicon oxide film according to claim 5, It is characterized in that The average thickness of silicon oxide film satisfies the following formula: D = (t1 + ... + tn) * v / n; Wherein, D is the average thickness of the silicon oxide film; t1 is the total corrosion time obtained when one bubble appears on the surface of the silicon wafer to be tested, and tn is the total corrosion time obtained when n bubbles appear on the surface of the silicon wafer to be tested, where n is greater than or equal to 2; v is the corrosion rate.
9. The method for testing the thickness of a silicon oxide film according to claim 5, It is characterized in that The thickness of the silicon oxide film satisfies the following formula: Dm=tm*v; Wherein, Dm is the thickness of the silicon oxide film at (Xm, Ym); (Xm, Ym) is the position where the mth bubble appears on the surface of the silicon wafer to be tested; tm is the corresponding total corrosion time obtained when the mth bubble appears on the surface of the silicon wafer to be tested; v is the corrosion rate.
10. The method for testing the thickness of a silicon oxide film according to any one of claims 5 to 9, It is characterized in that The silicon oxide film includes a tunneling silicon oxide film.