Clean preparation method of machine-made charcoal
Through a cleaning preparation method of mechanical charcoal, the problem of harmful gases and waste liquid treatment in the straw carbonization process is solved, efficient resource utilization and environmentally friendly production are achieved, and production costs and environmental pollution are reduced.
Patent Information
- Application Number
- CN202411076117.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The existing straw carbonization process produces a large number of harmful gases and waste liquids during the carbonization process, resulting in increased environmental pollution and production costs, and is not suitable for industrial production.
A cleaning preparation method of mechanical charcoal is adopted, including raw material pretreatment, drying, extrusion molding, carbonization, comprehensive treatment of waste gas and waste liquid, carbonization is carried out through high temperature and high pressure conditions in the carbonization kiln, and the use of waste gas and waste liquid Secondary utilization includes cooling, dust removal, condensation and activated carbon adsorption to achieve effective treatment of waste gas and waste liquid.
It has achieved high density and high hardness mechanical charcoal preparation, which has reduced the cost of hazardous waste treatment, improved resource utilization, reduced waste production, reduced production costs, and avoided environmental pollution, which is in line with the concept of green environmental protection.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of agricultural resources, and in particular to a clean preparation method of machine-made charcoal. Background Art
[0002] Machine-made charcoal, also known as machine-made charcoal, firewood sticks, artificial charcoal, regenerated charcoal, smokeless clean charcoal, has a wide range of raw materials. Rice husks, peanut shells, cotton shells, corn cobs, corn stalks, sorghum stalks, etc. can all be used as raw materials to produce charcoal sticks. Sawdust, wood shavings, and bamboo chips are the best. Because machine-made charcoal is smokeless, odorless, and non-toxic, it has been widely used in home heating and barbecue food; in the industrial field, it can be used as an industrial raw material and processed into activated carbon. Because machine-made charcoal has a high density, high calorific value, is smokeless, odorless, pollution-free, non-explosive, and flammable, it is an internationally recognized green and environmentally friendly product.
[0003] The difference between machine-made charcoal and other charcoal is: 1. Environmental protection: No trees are cut down, and waste from bamboo and wood products is used to produce it, turning waste into treasure. The production of ordinary charcoal requires cutting down trees, which damages the ecological environment.
[0004] 2. High energy: The fixed carbon content is about 80%, and the calorific value is 7500-8000kcal / kg, while the fixed carbon content of charcoal is low, and the calorific value is about 6500kcal / kg.
[0005] 3. Clean and hygienic: no smoke, no charcoal heads, no sparks during combustion, the residual ash falls naturally during combustion and does not float up, the ash content is about 3% or 6%, there is little residual ash after combustion, and it is flammable.
[0006] 4. Regular shape, reasonable structure, easy to use: uniform length and size, hollow or solid structure, conducive to burning and use.
[0007] 5. Low moisture content, within 5%: Ordinary charcoal has a high moisture content.
[0008] 6. The product does not contain chemicals, is non-toxic, odorless, pollution-free, and has a long burning time.
[0009] The method of preparing machine-made charcoal is to use sawdust as raw materials, dry them in a drying furnace to become standard raw materials with appropriate humidity, cool them down and put them into a molding machine (rod making machine), and then plasticize them at high temperature and high pressure to make firewood sticks (semi-finished products), and then carbonize them in a carbonization furnace. The purpose of using extrusion molding equipment is to shape raw materials containing a certain amount of water, so as to facilitate later carbonization or directly use them as firewood stick fuel. The manufacture of machine-made charcoal is mainly made of the carbon-containing components of the raw materials, such as cellulose and lignin. From the structural composition of the raw materials, there are two factors that determine whether it can become an ideal raw material for machine-made charcoal: the quality of cellulose bonding and the amount of lignin. The quality of cellulose bonding directly affects the density and mechanical strength of the molded stick, while the lignin content determines the maximum carbon content of the finished product. The chemical composition of cellulose and lignin used belongs to the category of carbohydrates. At the molecular level, they contain many hydrophilic groups, such as glucose, which constitutes its basic unit, and many hydroxyl groups. These hydrophilic groups are affinitive to many water molecules. During the extrusion process, if the temperature is too low, the lignin cannot be effectively softened to increase the viscosity, which is not conducive to high-pressure molding, and the water cannot be effectively discharged. The extruded firewood sticks are curved or not formed, which affects the subsequent carbonization and the yield of fixed carbon; if the temperature is too high, the lignin softens too quickly, the stick speed is fast, the firewood sticks are not strong, and the water will evaporate quickly into water vapor, leaving these hydrophilic groups, so that the firewood sticks burst, which is a manifestation of strong water loss of firewood sticks. The bursting or fractured lines of firewood sticks are not conducive to the later carbonization. At the same time, the extrusion temperature is too high, which also affects the cost of the product and the conditions for the molding machine. Therefore, in the process of extrusion and plasticization into firewood sticks, the selection of raw materials and the extrusion temperature are the two key parameters in the process of making mechanism charcoal.
[0010] Peanut shells are the shells of peanuts. Peanut shells are very common in rural areas, but the value of peanuts is mainly reflected in the seeds inside the peanut shells, and the practical value of the shells is relatively limited. Peanut shells contain nearly 60% crude fiber, ranking first among roughage. The dry matter in the nutritional components of peanut shells accounts for 90.3%, including 4.8% to 7.2% crude protein, 1% to 1.1% crude fat, 65.7% to 79.3% crude cellulose, 10.1% hemicellulose, and 10.6% to 21.2% soluble carbohydrates. In addition, peanut shells also contain vitamins, minerals and some amino acids. Most farmers treat them as garbage, some burn them directly, and some even throw them away directly, failing to make good use of peanut shells, resulting in a waste of resources.
[0011] After searching, the Chinese invention patent with application number "CN202111056310.1" discloses a straw carbonization process, including the following steps: straw pretreatment, straw high-temperature carbonization treatment, waste gas pretreatment, waste gas waste heat utilization and waste gas combustion utilization, and the carbonized straw and RDF are treated in a gasifier to generate usable gas. The present invention does not discharge waste gas to the outside during the entire production process, can absorb and treat harmful substances in the waste gas, and utilize the combustible gas in the waste gas. The method of recycling waste gas and re-burning enables the carbonization furnace to stabilize the heat. After two hours of external heating, it does not need to be heated. At the same time, it can operate normally for 4 to 5 hours, keeping the temperature in the furnace at 1300 degrees, saving resources and costs, and reasonably exchanging the waste heat in the waste gas to achieve effective recovery of waste heat. The waste heat gas generated by the final combustion is recovered through a pipeline for other uses, which plays a role in reasonable utilization of heat and energy saving.
[0012] However, the above-mentioned straw carbonization process method will produce a large amount of harmful gases and waste liquids during the straw carbonization process. The direct discharge of harmful gases without treatment will pollute the atmospheric environment. The management and harmless treatment of harmful gases and waste liquids as hazardous wastes will greatly increase production costs and are not suitable for industrial production. At the same time, the direct treatment of organic matter in the waste liquid is also a waste of resources.
[0013] In summary, there is an urgent need for a clean preparation method for machine-made charcoal to solve the above problems. Summary of the invention
[0014] In view of the shortcomings of the prior art, the present invention provides the above-mentioned straw carbonization process method. During the straw carbonization process, a large amount of harmful gases and waste liquids will be generated. The direct discharge of harmful gases without treatment will pollute the atmospheric environment. The management of waste liquids as hazardous wastes and harmless treatment will increase production costs, which is not suitable for industrial production and will also cause the problem of waste of resources.
[0015] To achieve the above object, the present invention provides the following technical solution: a clean preparation method of machine-made charcoal, comprising the following steps:
[0016] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0017] S2 drying, drying the crushed peanut shell powder until the moisture content is 10% to 13%;
[0018] S3 mechanism: The temperature in the rod making machine is heated to 140-160°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0019] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the internal pressure is maintained at 3-5MPa;
[0020] S4.1 Dehydration: The furnace temperature is slowly raised to 50-60°C at a rate of 3°C / min and kept at this temperature for 20-30 hours;
[0021] S4.2 Pyrolysis: The furnace temperature is slowly raised to 150-300°C at a rate of 5°C / min and kept at this temperature for 20-30h;
[0022] S4.3 Dehydrogenation and thermal condensation: The furnace temperature is slowly increased to 300-500°C at a rate of 10°C / min and kept at this temperature for 20-30h;
[0023] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is cooled naturally in the carbonization kiln to obtain the final product;
[0024] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0025] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas;
[0026] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is further cooled while the dust is removed;
[0027] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0028] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0029] S5.5 Waste gas combustion;
[0030] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0031] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0032] S7 waste treatment and utilization:
[0033] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0034] As a preferred embodiment of the clean preparation method of machine-made charcoal described in the present invention, the drying temperature in S2 is 120-140°C.
[0035] As a preferred embodiment of the clean preparation method of machine-made charcoal described in the present invention, the cooling time in S4.4 is 60 to 84 hours.
[0036] As a preferred embodiment of the clean preparation method of machine-made charcoal described in the present invention, the sum of the time of S4.1, S4.2 and S4.3 is 72 hours.
[0037] As a preferred solution of the clean preparation method of machine-made charcoal described in the present invention, the water heated by the heat exchanger in S5.1 is used for drying in S2.
[0038] As a preferred solution of the clean preparation method of machine-made charcoal described in the present invention, the waste gas after dust removal is transported to the interior of the carbonization kiln, and the waste gas is ignited to achieve fuel replenishment for the carbonization kiln and ensure a constant internal temperature.
[0039] As a preferred solution of the clean preparation method of machine-made charcoal described in the present invention, the waste gas after dust removal is burned to generate electricity with waste heat.
[0040] Compared with the prior art, the technical solution of this application has the following beneficial effects:
[0041] 1. The present invention discloses a clean preparation method for machine-made charcoal. The heating temperature in a rod-making machine is set to 140-160° C. The dried peanut shell powder is put into the rod-making machine in batches for extrusion and rod-making. The molding temperature of 140-160° C. softens the lignin component in the peanut shell powder and enhances the bonding ability. Coupled with the high-strength extrusion of the rod-making machine, a high-density and high-hardness molded carbon rod is finally obtained, which realizes the transformation of peanut shells into treasure and improves the utilization rate of agricultural products.
[0042] 2. The present invention discloses a clean preparation method for machine-made charcoal. Since the machine-made charcoal generated from peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation, the waste liquid mainly includes wood tar and wood vinegar. The waste liquid is cooled by a pipeline, and a mixture of wood tar and wood vinegar is formed after condensation. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification. The wood tar and wood vinegar are effectively utilized and processed, which can reduce the treatment cost of hazardous waste, realize the secondary utilization of hazardous waste, improve the rate of return, reduce production costs, and benefit large-scale production in factories.
[0043] 3. The present invention discloses a method for cleanly preparing machine-made charcoal. The machine-made charcoal prepared in the present application is used as activated carbon to absorb nitrogen oxides and sulfides. The discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, the discarded machine-made charcoal is placed inside a carbonization kiln and ignited to replenish the fuel of the carbonization kiln and ensure a constant temperature inside. This not only realizes the recycling of discarded machine-made charcoal, but also reduces the waste output of machine-made charcoal, thereby reducing waste treatment costs. At the same time, it avoids the large-scale purchase of activated carbon and reduces production costs.
[0044] 4. The present invention demonstrates a clean preparation method of machine-made charcoal. Since the exhaust gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas, a comprehensive dust treatment method of spraying + electrostatic + bag dust removal is used for the exhaust gas to reduce the dust content in the exhaust gas, avoid the possibility of dust explosion when the waste is reused, and improve production safety.
[0045] 5. The present invention shows a clean preparation method of machine-made charcoal, which realizes fuel replenishment of the carbonization kiln by arranging the wood gas inside the exhaust gas to be transported to the inside of the carbonization kiln, igniting the exhaust gas, ensuring a constant internal temperature, or burning the exhaust gas after dust removal for waste heat power generation, thereby realizing secondary waste utilization of the exhaust gas and improving the utilization efficiency; at the same time, activated carbon is adsorbed on the exhaust gas after combustion, thereby avoiding nitrogen oxides and sulfides from being directly discharged into the atmosphere and polluting the air, which is in line with the green and environmentally friendly production concept.
[0046] 6. The clean preparation method of machine-made charcoal demonstrated by the present invention realizes heat exchange with cooling water in the heat exchanger by arranging the exhaust gas to be transported into the heat exchanger, thereby cooling the exhaust gas. The water after heat exchange in the heat exchanger is used for drying, thereby realizing the utilization of exhaust gas and waste heat, reducing production costs and avoiding energy waste. DETAILED DESCRIPTION
[0047] First of all, it should be pointed out that in the different described embodiments, the same parts are provided with the same reference numerals or the same component names, wherein the disclosure contained in the entire description can be transferred to the same parts with the same reference numerals or the same component names. Selected positional descriptions in the description, such as top, bottom, lateral, etc., also refer to the directly described and shown ones and are transferred to the new positions in the case of a change in position.
[0048] Embodiment 1:
[0049] A clean preparation method for machine-made charcoal comprises the following steps:
[0050] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0051] S2 drying, drying the crushed peanut shell powder at a drying temperature of 120° C. until the moisture content is 13%;
[0052] S3 mechanism: The temperature in the rod making machine is heated to 140°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0053] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 3MPa;
[0054] S4.1 Dehydration: The furnace temperature is slowly raised to 50°C at a rate of 3°C / min and kept at this temperature for 24 hours;
[0055] S4.2 Pyrolysis: The furnace temperature was slowly raised to 150°C at a rate of 5°C / min and kept at this temperature for 24h;
[0056] S4.3 Dehydrogenation and thermal condensation: The furnace temperature is slowly increased to 300°C at a rate of 10°C / min and kept at this temperature for 24 hours;
[0057] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is naturally cooled in the carbonization kiln for 60 hours to obtain the final product;
[0058] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0059] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; the water after heat exchange in the heat exchanger is used for drying;
[0060] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is cooled while the dust is removed;
[0061] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0062] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0063] S5.5 Waste gas combustion: The waste gas after dust removal is transported to the interior of the carbonization kiln, where it is ignited to replenish the fuel of the carbonization kiln or burned for waste heat power generation.
[0064] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0065] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0066] Wood vinegar, also known as plant acid, is a reddish-brown liquid obtained after the steam-gas mixture derived from the dry distillation of wood and other biomass in the dry distillation equipment is condensed and separated. It is a mixture with very complex components. The wood vinegar obtained directly from the dry distillation condensation equipment is called crude wood vinegar, which is a brown-black liquid containing a large amount of tar and harmful substances, etc., and needs to be further refined according to different uses. The crude wood vinegar obtained by the dry distillation of biomass is separated into two layers when left to stand and clarify, the upper layer is clarified wood vinegar, and the lower layer is precipitated wood tar. Further processing of clarified wood vinegar can obtain products such as acetic acid (or acetate), propionic acid, butyric acid, methanol and organic solvents. After processing, precipitated wood tar can obtain products such as creosote, creosote, wood tar anti-agglomeration agent, wood asphalt, etc.
[0067] Wood tar is a high temperature resistant material, with a high temperature resistance of up to 280°C. It is waterproof and is an excellent material for corrosion resistance and high temperature resistance in the shipbuilding industry and paint industry. It is a chemical and pharmaceutical raw material and plant nutrition regulator, which has a growth effect on plants and is excellent in killing insects.
[0068] S7 waste treatment and utilization:
[0069] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0070] Embodiment 2:
[0071] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0072] S2 drying, drying the crushed peanut shell powder at a drying temperature of 140° C. until the moisture content is 10%;
[0073] S3 mechanism: The temperature in the rod making machine is heated to 160°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0074] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 5MPa;
[0075] S4.1 Dehydration: The furnace temperature is slowly raised to 60°C at a rate of 3°C / min and kept at this temperature for 20 hours;
[0076] S4.2 Pyrolysis: The furnace temperature is slowly increased to 300°C at a rate of 5°C / min and kept at this temperature for 30h;
[0077] S4.3 Dehydrogenation and thermal condensation: the furnace temperature is slowly increased to 500°C at a rate of 10°C / min and kept at this temperature for 22 hours;
[0078] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is naturally cooled in the carbonization kiln for 84 hours to obtain the final product;
[0079] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0080] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; the water after heat exchange in the heat exchanger is used for drying;
[0081] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is cooled while the dust is removed;
[0082] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0083] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0084] S5.5 Waste gas combustion: the waste gas after dust removal is transported to the inside of the carbonization kiln, and the waste gas is ignited to realize the fuel replenishment of the carbonization kiln, or burned for waste heat power generation;
[0085] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0086] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0087] S7 waste treatment and utilization:
[0088] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0089] Embodiment three:
[0090] A clean preparation method for machine-made charcoal comprises the following steps:
[0091] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0092] S2 drying, drying the crushed peanut shell powder at a drying temperature of 130° C. until the moisture content is 12%;
[0093] S3 mechanism: The temperature in the rod making machine is heated to 130°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0094] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 4MPa;
[0095] S4.1 Dehydration: The furnace temperature is slowly raised to 55°C at a rate of 3°C / min and kept at this temperature for 30 hours;
[0096] S4.2 Pyrolysis: The furnace temperature was slowly raised to 250°C at a rate of 5°C / min and kept at this temperature for 20 h;
[0097] S4.3 Dehydrogenation and thermal condensation: the furnace temperature is slowly increased to 400°C at a rate of 10°C / min and kept at this temperature for 22 hours;
[0098] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is naturally cooled in the carbonization kiln for 72 hours to obtain the final product;
[0099] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0100] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; the water after heat exchange in the heat exchanger is used for drying;
[0101] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is cooled while the dust is removed;
[0102] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0103] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0104] S5.5 Waste gas combustion: the waste gas after dust removal is transported to the inside of the carbonization kiln, and the waste gas is ignited to realize the fuel replenishment of the carbonization kiln, or burned for waste heat power generation;
[0105] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0106] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0107] S7 waste treatment and utilization:
[0108] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0109] Embodiment 4:
[0110] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0111] S2 drying, drying the crushed peanut shell powder at a drying temperature of 140° C. until the moisture content is 12%;
[0112] S3 mechanism: The temperature in the rod making machine is heated to 160°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0113] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 5MPa;
[0114] S4.1 Dehydration: The furnace temperature is slowly raised to 60°C at a rate of 3°C / min and kept at this temperature for 24 hours;
[0115] S4.2 Pyrolysis: The furnace temperature is slowly increased to 300°C at a rate of 5°C / min and kept at this temperature for 28h;
[0116] S4.3 Dehydrogenation and thermal condensation: the furnace temperature is slowly increased to 500°C at a rate of 10°C / min and kept at this temperature for 20 hours;
[0117] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is naturally cooled in the carbonization kiln for 84 hours to obtain the final product;
[0118] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0119] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; the water after heat exchange in the heat exchanger is used for drying;
[0120] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is cooled while the dust is removed;
[0121] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0122] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0123] S5.5 Waste gas combustion: the waste gas after dust removal is transported to the inside of the carbonization kiln, and the waste gas is ignited to realize the fuel replenishment of the carbonization kiln, or burned for waste heat power generation;
[0124] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0125] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0126] S7 waste treatment and utilization:
[0127] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0128] Embodiment five:
[0129] S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder;
[0130] S2 drying, drying the crushed peanut shell powder at a drying temperature of 140° C. until the moisture content is 12%;
[0131] S3 mechanism: The temperature in the rod making machine is heated to 160°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making;
[0132] S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 4MPa;
[0133] S4.1 Dehydration: The furnace temperature is slowly raised to 60°C at a rate of 3°C / min and kept at this temperature for 22 hours;
[0134] S4.2 Pyrolysis: The furnace temperature is slowly increased to 300°C at a rate of 5°C / min and kept at this temperature for 20h;
[0135] S4.3 Dehydrogenation and thermal condensation: the furnace temperature is slowly increased to 500°C at a rate of 10°C / min and kept at this temperature for 30 hours;
[0136] S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is naturally cooled in the carbonization kiln for 84 hours to obtain the final product;
[0137] S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused;
[0138] S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; the water after heat exchange in the heat exchanger is used for drying;
[0139] S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is cooled while the dust is removed;
[0140] S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal;
[0141] S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal;
[0142] S5.5 Waste gas combustion: the waste gas after dust removal is transported to the inside of the carbonization kiln, and the waste gas is ignited to realize the fuel replenishment of the carbonization kiln, or burned for waste heat power generation;
[0143] S5.6 Activated carbon adsorption: The machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides;
[0144] S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated;
[0145] S7 waste treatment and utilization:
[0146] On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply of the carbonization kiln.
[0147] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0148] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A clean preparation method for machine-made charcoal, Features: The following steps are involved: S1 Raw material pretreatment: crushing peanut shells to produce peanut shell powder; S2 drying, drying the crushed peanut shell powder until the moisture content is 10% to 13%; S3 mechanism: The temperature in the rod making machine is heated to 140-160°C, and the dried peanut shell powder is put into the rod making machine in batches for extrusion and rod making; S4 Carbonization: Carbonization kiln is used to carbonize the formed carbon rods, and the pressure is maintained at 3-5MPa; S4.1 Dehydration: The furnace temperature is slowly raised to 50-60°C at a rate of 3°C / min and kept at this temperature for 20-30 hours; S4.2 Pyrolysis: The furnace temperature is slowly raised to 150-300°C at a rate of 5°C / min and kept at this temperature for 20-30h; S4.3 Dehydrogenation and thermal condensation: The furnace temperature is slowly increased to 300-500°C at a rate of 10°C / min and kept at this temperature for 20-30h; S4.4 Cooling: After the carbon rod is completely carbonized, the heating is stopped, and the air inlet and outlet of the carbonization kiln are closed. The carbon rod is cooled naturally in the carbonization kiln to obtain the final product; S5 Waste gas treatment and utilization: The waste gas generated during the carbonization process is mainly composed of dust and combustible gases such as wood gas. The waste gas is cooled and dusted, and the waste gas is reused; S6 Waste liquid treatment and utilization: The machine-made charcoal generated by peanut shell powder will generate a large amount of waste liquid after dehydrogenation and thermal condensation. The waste liquid mainly includes water, wood tar and wood vinegar. The waste liquid is cooled by pipeline, and the waste liquid is condensed to form a mixture of wood tar and wood vinegar. The wood tar and wood vinegar are separated by dry distillation, condensation, and static stratification, and effectively utilized and treated; S7 waste treatment and utilization: On the one hand, the discarded machine-made charcoal is used as activated carbon to absorb nitrogen oxides and sulfides. On the other hand, it is placed inside the carbonization kiln and ignited to realize the fuel supply to the carbonization kiln.
2. A clean preparation method for machine-made charcoal according to claim 1, Features: The S5 comprises the following steps: S5.1 Cooling treatment: the exhaust gas is transported to the heat exchanger to achieve heat exchange with the cooling water in the heat exchanger, so as to utilize the waste heat of the exhaust gas and cool the exhaust gas; S5.2 Spraying dust removal: The exhaust gas enters the settling chamber for spraying, and the exhaust gas is further cooled while the dust is removed; S5.3 Electrostatic dust removal: The exhaust gas after spraying is subjected to electrostatic dust removal; S5.4 Bag dust removal: Settle the dust in the exhaust gas after electrostatic dust removal; S5.5 Waste gas combustion; S5.6 Activated carbon adsorption: The discarded machine-made charcoal prepared in this application is used as activated carbon to absorb nitrogen oxides and sulfides.
3. The clean preparation method of machine-made charcoal according to claim 1, Features: The drying temperature in S2 is 120-140°C.
4. The clean preparation method of machine-made charcoal according to claim 1, Features: The cooling time of S4.4 is 60 to 84 hours.
5. A clean preparation method for machine-made charcoal according to claim 4, Features: The preferred cooling time of S4.4 is 72 hours.
6. The clean preparation method of machine-made charcoal according to claim 1, Features: The total time of S4.1, S4.2 and S4.3 is 72 hours.
7. The clean preparation method of machine-made charcoal according to claim 2, Features: The water after heat exchange in the S5.1 heat exchanger is used for drying in the S2.
8. The clean preparation method of machine-made charcoal according to claim 2, Features: The waste gas after dust removal in S5.5 is transported to the interior of the carbonization kiln, and the waste gas is ignited to achieve fuel replenishment for the carbonization kiln and ensure a constant temperature inside.
9. The clean preparation method of machine-made charcoal according to claim 2, Features: The exhaust gas after dust removal in S5.5 is burned to generate electricity with waste heat.