Production method for rapidly slagging aluminum killed steel
By adopting high-purity aluminum blocks and online wire feeding technology in aluminum calming steel production, combined with the optimized calcium treatment system and CaO-Al2O3 slag system, the problems of Al2O3 inclusion removal and plug rod erosion in aluminum calming steel are solved, and the problem of Al2O3 inclusion removal and plug rod erosion in aluminum calming steel is achieved. The effect of precise aluminum control and reducing production costs is achieved.
Patent Information
- Application Number
- CN202410004031.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-02
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to accurately control aluminum during the production process, resulting in the formation of Al2O3 inclusions, affecting the continuous casting and casting process. The existing calcium treatment technology leads to serious erosion of the plug rod, increasing production costs and accident risks.
High-purity aluminum blocks are used to replace silicon-aluminum calcium for converter deoxygenation, online wire feeding technology is used to increase aluminum in LF furnaces, optimize the calcium treatment system to control Al2O3 denaturation and inclusion removal, and use CaO-Al2O3 slag system for slag making operation to improve Inclusion adsorption effect.
Accurate aluminum control, reduce production costs, improve the quality of white slag, extend the number of continuous pouring furnaces, reduce production accidents, reduce aluminum products consumption, and improve the low consumption and efficiency of calcium treatment.
Smart Images

Figure BDA0004645875700000041 
Figure BDA0004645875700000051 
Figure BDA0004645875700000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, in particular to a production method for rapid slag formation of aluminum killed steel. Background Art
[0002] Aluminum-killed steel is a metal material. If only Si+Mn is used for deoxidation, subcutaneous pinholes are easily formed in the ingot. In addition to using LF white slag refining to reduce [O]D in the steel, Si+Mn+a small amount of aluminum can also be used for deoxidation. However, if it is necessary to maintain the castability of continuous casting and prevent the ingot from producing subcutaneous pinholes, Si+Mn+a small amount of aluminum should be used for deoxidation. The deoxidation products formed may include: ① rhodonite (2MnO·2Al2O3·5SiO2); ② manganese aluminum garnet (3MnO·Al2O3·3SiO2); ③ pure (Al2O3>25%).
[0003] Aluminum-killed steel is a type of steel that removes excess oxygen by adding aluminum to the steel when it is tapped from a converter or electric furnace. The difficulties in producing this type of steel are: ① Aluminum plays a role in refining grains in steel and improving product performance, but aluminum is an easily oxidized element, difficulty 1-precise control of aluminum; ② Al2O3 generated by aluminum deoxidation is a high-melting-point inclusion. If it cannot be effectively removed, the water inlet will be blocked during the continuous casting process, resulting in production interruption, difficulty 2-floating removal of inclusions; ③ Calcium treatment technology is an effective means of degenerating Al2O3 inclusions. How to choose a suitable process system that can not only ensure that Al2O3 inclusions are degenerated into low-melting-point inclusions and removed, but also prevent excessive calcium content from corroding the stopper rod refractory, so as to increase the number of continuous casting furnaces, reduce production costs, and reduce production accidents, difficulty 3-calcium treatment system formulation.
[0004] In the existing technology, the converter currently uses silicon, aluminum and calcium for steelmaking deoxidation and alloying, and the LF furnace uses aluminum particles to increase aluminum or offline wire feeding, which cannot accurately control aluminum; the aluminum killed steel currently uses CaO-CaF2 slag system for slag making operations, CaF2 is harmful to the environment and corrodes refractory materials, and the slag system has a weak ability to adsorb Al2O3 inclusions; the aluminum killed steel continuous casting furnace currently uses a quantitative calcium treatment method, and the calcium treatment intensity is large, the stopper rod is severely eroded, and in severe cases, the crystallizer liquid level fluctuates, affecting the quality of the casting; in view of this, we propose a production method for rapid slag formation of aluminum killed steel. Summary of the invention
[0005] The object of the present invention is to provide a method for producing rapid slag formation of aluminum killed steel to solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for producing aluminum killed steel rapid slag, the method comprising the following steps:
[0007] Step 1: Precisely control aluminum processing:
[0008] Step 11, the converter uses high-purity aluminum blocks to replace silicon-aluminum-calcium for deoxidation operation, and the aluminum blocks are added according to the carbon content of the steel;
[0009] Step 12: LF aluminum wire adopts online wire feeding technology, instead of using aluminum pellets to increase aluminum or offline wire feeding, to accurately control aluminum;
[0010] Step 2: Remove Al2O3 inclusions:
[0011] Step 21, treating the carbon content of the steel produced from the converter;
[0012] Step 22, endpoint carbon treatment, top slag addition treatment;
[0013] Step 23, LF furnace slag making process;
[0014] Step 24, LF furnace deoxidation process;
[0015] Step 25, the white residue is kept waiting for processing;
[0016] Step 26: soft blowing treatment;
[0017] Step 27, LF furnace final slag target: FeO+MnO≤1%, CaO: 40%-60%, Al2O3: 20%-35%, SiO2≤10%;
[0018] Step 3: Establish calcium treatment system.
[0019] Optionally, the control target of the carbon content treatment of the steel in step 21 is 0.10%-0.30%.
[0020] Optionally, in the step 22, 1.1 kg / t steel of pre-melted refined slag and 4.5 kg / t steel of lime are added during the steel tapping process of the converter.
[0021] Optionally, step 23 further includes: adding lime at 0-1.1 kg / t steel and pre-melted refined slag at 0.2-0.4 kg / t steel during the refining process.
[0022] Optionally, the step 24 further comprises: adding 0.1-0.6 kg / t steel of aluminum particles and 0.2-1.1 kg / t steel of calcium carbide during the refining process, adding deoxidizer in batches during the heating gap, and performing slag dipping operation each time the heating is stopped;
[0023] If it turns white, it is considered that the white slag is well made;
[0024] Otherwise, continue to sprinkle deoxidizer.
[0025] Optionally, the step 25 further comprises: keeping the white slag in the waiting process for ≥10 min.
[0026] Optionally, the soft blowing time of the soft blowing treatment in step 26 is ≥15 min.
[0027] Optionally, step 3 further includes: a wire feeding speed of 120 m / min, a reference wire feeding amount of the first furnace of 3.3±0.4 (m / t steel), and a reference wire feeding amount of the continuous casting furnace of 0.8±0.4 (m / t steel).
[0028] Compared with the prior art, the present invention provides a method for producing aluminum killed steel by rapid slag formation, which has the following beneficial effects:
[0029] 1. The production method of rapid slag formation of aluminum-killed steel adopts aluminum blocks instead of silicon, aluminum and calcium for converter steel deoxidation, thereby reducing production costs; the LF furnace uses online aluminum replenishment technology to replace aluminum particle replenishment operation and offline aluminum replenishment, thereby ensuring accurate aluminum replenishment of the LF furnace and reducing the consumption of aluminum products; the LF furnace adopts CaO-Al2O3 slag system for slag making operation, thereby improving the adsorption effect of inclusions.
[0030] 2. The production method of rapid slag formation of aluminum-killed steel optimizes the deoxidation system of the LF furnace, adds deoxidizer in small batches in multiple batches, improves the deoxidation effect, and improves the quality of white slag; provides a calcium treatment system to ensure that the low consumption requirements are met on the basis of Al2O3 modification, increase the number of continuous casting furnaces, and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the process structure of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] like Figure 1 As shown, the present invention provides a technical solution: a production method for rapid slag formation of aluminum killed steel, comprising the following steps:
[0035] S1. Precise control of aluminum processing:
[0036] S11. The converter uses high-purity aluminum blocks to replace silicon, aluminum and calcium for deoxidation operation. Aluminum blocks are added according to the carbon content of the steel, and the amount of aluminum blocks added is shown in the following table:
[0037]
[0038] S12 and LF aluminum wires use online wire feeding technology, which replaces the use of aluminum particles for aluminum addition or offline wire feeding, to achieve the purpose of precise aluminum control.
[0039] In this embodiment, aluminum blocks are used instead of silicon, aluminum and calcium for converter steel deoxidation to reduce production costs; the LF furnace uses online aluminum replenishment technology to replace aluminum particle replenishment operations and offline aluminum replenishment to ensure accurate aluminum replenishment in the LF furnace and reduce the consumption of aluminum products; the LF furnace uses CaO-Al2O3 slag system for slag making operations to improve the adsorption effect of inclusions.
[0040] S2. Remove Al2O3 inclusions:
[0041] S21, the carbon content of the converter steel is controlled at 0.10%;
[0042] S22, final carbon treatment, top slag addition treatment, adding pre-melted refined slag 1.1kg / t steel, lime 4.5kg / t steel during converter tapping;
[0043] S23, LF furnace slag making process, add lime 0.2kg / t steel, pre-melting type refined slag 0.2kg / t steel during refining process, and the viscosity of slag can be adjusted appropriately;
[0044] S24, LF furnace deoxidation process, add aluminum particles 0.1kg / t steel, calcium carbide 0.2kg / t steel during the refining process, add deoxidizer in batches during the heating interval, and perform slag dipping operation every time the heating is stopped. If it turns white, it is considered that the white slag is ready, otherwise continue to sprinkle the deoxidizer;
[0045] S25, white slag is kept waiting for treatment, and the white slag holding time is ≥10min;
[0046] S26, soft blowing treatment, and the soft blowing time is ≥ 15min;
[0047] S27, LF furnace final slag target: FeO+MnO≤1%, CaO: 40%-60%, Al2O3: 20%-35%, SiO2≤10%.
[0048] S3. Calcium treatment system formulation: The results of the calcium treatment system formulation are shown in the following table:
[0049]
[0050] Among them, the Ca / AL ratio is: 0.05-0.15. It can ensure that the low consumption requirements are met on the basis of Al2O3 modification, increase the number of continuous casting furnaces, and reduce production costs; in addition, the LF furnace deoxidation system is optimized, and deoxidizers are added in small batches in multiple batches to improve the deoxidation effect and improve the quality of white slag; a calcium treatment system is provided to ensure that the low consumption requirements are met on the basis of Al2O3 modification, increase the number of continuous casting furnaces, and reduce production costs.
[0051] Embodiment 2:
[0052] like Figure 1 As shown, the present invention provides a technical solution: a production method for rapid slag formation of aluminum killed steel, comprising the following steps:
[0053] S1. Precise control of aluminum processing:
[0054] S11. The converter uses high-purity aluminum blocks to replace silicon, aluminum and calcium for deoxidation operation. Aluminum blocks are added according to the carbon content of the steel, and the amount of aluminum blocks added is shown in the following table:
[0055]
[0056] S12 and LF aluminum wires use online wire feeding technology, which replaces the use of aluminum particles for aluminum addition or offline wire feeding, to achieve the purpose of precise aluminum control.
[0057] S2. Remove Al2O3 inclusions:
[0058] S21, the carbon content of the converter steel is controlled at 0.25%;
[0059] S22, final carbon treatment, top slag addition treatment, adding pre-melted refined slag 1.1kg / t steel, lime 4.5kg / t steel during converter tapping;
[0060] S23, LF furnace slag making process, add lime 0.6kg / t steel, pre-melting type refined slag 0.3kg / t steel during the refining process, and the viscosity of the added slag can be appropriately adjusted;
[0061] S24, LF furnace deoxidation process, add aluminum particles 0.4kg / t steel, calcium carbide 0.7kg / t steel during the refining process, add deoxidizer in batches during the heating interval, and dip the slag every time the heating is stopped. If it turns white, it is considered that the white slag is ready, otherwise continue to sprinkle the deoxidizer;
[0062] S25, white slag is kept waiting for treatment, and the white slag holding time is ≥10min;
[0063] S26, soft blowing treatment, and the soft blowing time is ≥ 15min;
[0064] S27, LF furnace final slag target: FeO+MnO≤1%, CaO: 40%-60%, Al2O3: 20%-35%, SiO2≤10%.
[0065] S3. Calcium treatment system formulation: The results of the calcium treatment system formulation are shown in the following table:
[0066]
[0067] In this embodiment, the Ca / AL ratio is: 0.11.
[0068] Embodiment three:
[0069] like Figure 1 As shown, the present invention provides a technical solution: a production method for rapid slag formation of aluminum killed steel, comprising the following steps:
[0070] S1. Precise control of aluminum processing:
[0071] S11. The converter uses high-purity aluminum blocks to replace silicon, aluminum and calcium for deoxidation operation. Aluminum blocks are added according to the carbon content of the steel, and the amount of aluminum blocks added is shown in the following table:
[0072]
[0073] S12 and LF aluminum wires use online wire feeding technology, which replaces the use of aluminum particles for aluminum addition or offline wire feeding, to achieve the purpose of precise aluminum control.
[0074] In this embodiment, aluminum blocks are used instead of silicon, aluminum and calcium for converter steel deoxidation to reduce production costs; the LF furnace uses online aluminum replenishment technology to replace aluminum particle replenishment operations and offline aluminum replenishment to ensure accurate aluminum replenishment in the LF furnace and reduce the consumption of aluminum products; the LF furnace uses CaO-Al2O3 slag system for slag making operations to improve the adsorption effect of inclusions.
[0075] S2. Remove Al2O3 inclusions:
[0076] S21, the carbon content of the converter steel is controlled at 0.30%;
[0077] S22, final carbon treatment, top slag addition treatment, adding pre-melted refined slag 1.1kg / t steel, lime 4.5kg / t steel during converter tapping;
[0078] S23, LF furnace slag making process, add lime 1.1kg / t steel, pre-melting type refined slag 0.2-0.4kg / t steel during the refining process, and the viscosity of the added slag can be adjusted appropriately;
[0079] S24, LF furnace deoxidation process, add aluminum particles 0.6kg / t steel, calcium carbide 1.1kg / t steel during the refining process, add deoxidizer in batches during the heating interval, and dip the slag every time the heating is stopped. If it turns white, it is considered that the white slag is ready, otherwise continue to sprinkle the deoxidizer;
[0080] S25, white slag is kept waiting for treatment, and the white slag holding time is ≥10min;
[0081] S26, soft blowing treatment, and the soft blowing time is ≥ 15min;
[0082] S27, LF furnace final slag target: FeO+MnO≤1%, CaO: 40%-60%, Al2O3: 20%-35%, SiO2≤10%.
[0083] S3. Calcium treatment system formulation: The results of the calcium treatment system formulation are shown in the following table:
[0084]
[0085] In this embodiment, the Ca / AL ratio is 0.15. It can ensure that the low consumption requirement is met on the basis of Al2O3 modification, increase the number of continuous casting furnaces, and reduce production costs; in addition, the LF furnace deoxidation system is optimized, and deoxidizers are added in small batches in multiple batches to improve the deoxidation effect and improve the quality of white slag; a calcium treatment system is provided to ensure that the low consumption requirement is met on the basis of Al2O3 modification, increase the number of continuous casting furnaces, and reduce production costs.
[0086] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.
Claims
1. A method for producing aluminum killed steel by rapid slag formation, Features: The method comprises the following steps: Step 1: Precisely control aluminum processing: Step 11, the converter uses high-purity aluminum blocks to replace silicon-aluminum-calcium for deoxidation operation, and the aluminum blocks are added according to the carbon content of the steel; Step 12: LF aluminum wire adopts online wire feeding technology, instead of using aluminum pellets to increase aluminum or offline wire feeding, to accurately control aluminum; Step 2: Al 2 O 3 Inclusion removal treatment: Step 21, treating the carbon content of the steel produced from the converter; Step 22, endpoint carbon treatment, top slag addition treatment; Step 23, LF furnace slag making process; Step 24, LF furnace deoxidation process; Step 25, the white residue is kept waiting for processing; Step 26: soft blowing treatment; Step 27, LF furnace final slag target: FeO+MnO≤1%, CaO: 40%-60%, Al 2 O 3 :20%-35%, SiO2≤10%; Step 3: Establish calcium treatment system.
2. The method for producing aluminum killed steel by rapid slag formation according to claim 1, Features: The control target of the carbon content treatment of the steel in step 21 is 0.10%-0.30%.
3. The method for producing aluminum killed steel by rapid slag formation according to claim 1, Features: In the step 22, 1.1 kg / t steel of pre-melted refined slag and 4.5 kg / t steel of lime are added during the steel tapping process of the converter.
4. The method for producing aluminum killed steel by rapid slag formation according to claim 1, Features: The step 23 further comprises: adding lime 0-1.1 kg / t steel and pre-melted refined slag 0.2-0.4 kg / t steel during the refining process.
5. The method for producing aluminum killed steel rapid slag according to claim 1, Features: The step 24 further comprises: adding 0.1-0.6 kg / t steel of aluminum particles and 0.2-1.1 kg / t steel of calcium carbide during the refining process, adding deoxidizer in batches during the heating gap, and performing slag dipping operation each time the heating is stopped; If it turns white, it is considered that the white slag is well made; Otherwise, continue to sprinkle deoxidizer.
6. The method for producing aluminum killed steel rapid slag according to claim 1, Features: The step 25 further comprises: keeping the white slag in the waiting process for ≥10 minutes.
7. The method for producing aluminum killed steel rapid slag according to claim 1, Features: The soft blowing time of the soft blowing treatment in step 26 is ≥15 min.
8. The method for producing aluminum killed steel rapid slag according to claim 1, Features: The step 3 further includes: the wire feeding speed is 120m / min, the reference wire feeding amount of the first furnace is 3.3±0.4 (m / t steel), and the reference wire feeding amount of the continuous casting furnace is 0.8±0.4 (m / t steel).