Method for smelting low-phosphorus stainless steel by using stainless steel iron oxide ball

By using stainless steel iron oxide balls and nitrogen spray lime powder in blast furnace molten iron, FeO is used to accelerate the dephosphorization reaction, the problem of low dephosphorization rate of low phosphorus stainless steel in the existing smelting process is solved, and high-efficiency phosphorus content is achieved Reduction and cost reduction have significantly improved the quality of steel products.

CN118996053APending Publication Date: 2024-11-22GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205579.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing smelting process is difficult to effectively improve the dephosphorization rate of low-phosphorus stainless steel in blast furnace molten iron, resulting in difficulty in reducing the phosphorus content and affecting the mechanical properties of steel products.

Method used

The stainless steel iron oxide ball smelting method is adopted. By adding the stainless steel iron oxide ball to the blast furnace molten iron, the high-oxidation substance FeO is used to accelerate the dephosphorization reaction, and deep dephosphorization smelting is carried out in combination with nitrogen spray lime powder to gradually reduce the phosphorus content.

Benefits of technology

The dephosphorization rate of low-phosphorus stainless steel has been significantly improved, smelting costs have been reduced, the quality of steel products has been improved, and the operation has been kept simple and the existing production model has remained unchanged.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for smelting low-phosphorus stainless steel by using a stainless steel iron oxide ball. The method comprises the following steps: (1) preparing the stainless steel iron oxide ball; (2) transporting and feeding; (3) feeding molten iron in a three-removal smelting process; (4) blowing, dephosphorizing and smelting; (5) slagging off; (6) outbound; and after P in the molten iron is measured to be smaller than or equal to 0.010%, the molten iron is lifted out of a dephosphorization station, and finally the dephosphorized molten iron is added into an AOD converter to be subjected to decarburization and alloying operation. By means of the method, the self-produced stainless steel iron oxide ball of solid waste is added into the dephosphorization ladle through the overhead bunker for smelting, due to the fact that the stainless steel iron oxide ball contains much FeO, the oxidizing atmosphere can be provided for the ladle, the dephosphorization reaction is accelerated, the dephosphorization rate is increased, and the smelting cost of low-phosphorus stainless steel is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a method for smelting low-phosphorus stainless steel by utilizing stainless steel iron oxide balls. Background Art

[0002] China's steel production leads the world and is currently in a stage of rapid development from a steel power to a steel power. Many steelmaking technologies are leading in the world. The key indicator for judging the quality of steel is the phosphorus content. The appropriate phosphorus content can increase the strength of steel, but for most steels, phosphorus is a harmful element. High phosphorus content will reduce the plasticity of steel, weldability and impact toughness. Studies have shown that during the solidification of molten steel, phosphorus segregation is concentrated at the grain boundary, causing the brittleness of steel in a low temperature environment. This phenomenon is called "cold brittleness". The phosphorus content has a great impact on steel, so that a very small amount of phosphorus (0.010%) can also cause low-temperature brittleness of steel. Although the existing process cannot completely remove phosphorus from steel, reducing the phosphorus content in steel as much as possible can greatly improve the mechanical properties of steel. Based on this, the phosphorus content of ordinary steel is required to be less than 0.040%, and the phosphorus content of drilling platforms, ships, rails, steel bearing parts and liquefied gas pipelines in special cold areas should be less than 0.030%.

[0003] Iron oxide scale is an iron-containing oxide produced on the surface of steel after the rolled piece is rapidly cooled by water during rolling. It is a byproduct of steelmaking and is produced in large quantities. If the iron oxide scale can be used reasonably, it can not only reduce the cost of steelmaking production, but also play a role in environmental protection and energy saving. The main components of iron oxide scale are Fe0, Fe 2 0 3 , Fe 3 0 4 The removal of phosphorus in stainless steel smelting process mainly relies on oxidation dephosphorization method, that is, Fe0 in slag is oxidized with phosphorus dissolved in metal to generate P 2 O 5 Then it reacts with Ca0 in the slag to form stable calcium phosphate, which eventually enters the slag and is removed. Oxidative dephosphorization has gradually become a common method for smelting low-phosphorus stainless steel in the steel industry due to its high efficiency and low cost. How to effectively improve the dephosphorization rate of molten iron has become a key technical problem in smelting low-phosphorus stainless steel. Summary of the invention

[0004] The invention provides a method for smelting low-phosphorus stainless steel by using stainless steel iron oxide balls, aiming at improving the dephosphorization rate of the low-phosphorus stainless steel smelted by blast furnace molten iron.

[0005] To achieve its purpose, the present invention adopts the following technical solution: A method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls comprises the following steps: (1) Preparing stainless steel iron oxide balls; using clay as a binder, pressing the stainless steel iron oxide into balls, and drying them naturally or in an oven to obtain stainless steel iron oxide balls; the chemical composition of the stainless steel iron oxide balls is as follows: 4%≤Si0 2 ≤8%, Fe0≥45%, TFe≥55%, H 2 0≤5%; (2) transporting and loading materials; transporting the stainless steel iron oxide balls in step (1) to the third degassing warehouse, and lifting them to the silo by the bucket belt for standby use; (3) The hot metal from the three-removal smelting process enters the station; the hot metal from the blast furnace is added to the pre-treated hot metal ladle. The chemical composition of the hot metal is calculated by weight percentage as follows: C ≥ 4.0%, Si: 0.3-1.0%, Mn ≤ 1.0%, P ≤ 0.1%, and the rest is Fe and other uncontrollable elements brought from the raw materials; (4) dephosphorization by spraying; adding the stainless steel iron oxide balls in step (2) into the molten iron in the blast furnace in step (3), and using nitrogen as a carrier gas to spray lime powder for deep dephosphorization and triple dephosphorization; ① Desiliconization period: In the early stage of smelting, oxygen is blown for desiliconization, and lime powder is sprayed to make slag. When the silicon content is reduced to <0.27%, the desiliconized slag is poured out; ② Secondary slagging and dephosphorization: After pouring out part of the desiliconized slag, continue to blow oxygen for desiliconization, and re-blow lime powder to make slag for dephosphorization; (5) Slag removal: After dephosphorization, the high-phosphorus slag produced in the ladle is removed by a slag remover to remove at least 70%; (6) Exit the station: After the P content in the molten iron is measured to be ≤ 0.010%, the molten iron is hoisted out of the dephosphorization station; (7) The molten iron after dephosphorization in step (6) is added into the AOD converter for decarburization and alloying operations.

[0006] Furthermore, in step (1), the amount of clay used is 10-15wt% of the total weight of the stainless steel iron oxide ball.

[0007] Furthermore, in step (1), the diameter of the stainless steel iron oxide ball is 30-40 mm.

[0008] Furthermore, in step (3), the temperature of the molten iron in the blast furnace is 1280-1350°C.

[0009] Furthermore, in step (4), the amount of stainless steel iron oxide balls used is 50-100 kg / t molten iron, and the feeding speed of the stainless steel iron oxide balls is 80-160 kg / min.

[0010] Furthermore, in step (4), the amount of lime powder sprayed is 13-32 kg / t molten iron, and the spraying pressure is 0.30-0.40 MPa.

[0011] Furthermore, the oxygen flow rate of oxygen desiliconization during the desiliconization period in step (4) is 36-40m 3 / min; lime powder injection flow rate is 40-45m 3 / min, nitrogen flow rate is 2.3-2.5m 3 / min, the lime powder injection time is 8-15min.

[0012] Furthermore, in step (4), the oxygen flow rate during the secondary slag dephosphorization is 30-36m 3 / min; lime powder injection flow rate is 35-45m 3 / min, nitrogen flow rate is 2.3-2.5m 3 / min, dephosphorization alkalinity is 1.4-1.6, and lime powder injection time is 24-32min.

[0013] Furthermore, in step (6), all high-phosphorus slag is removed before the molten iron leaves the station.

[0014] The beneficial effects of the present invention are as follows: 1. The method for smelting low-phosphorus stainless steel using stainless steel oxidized iron balls provided by the present invention comprises adding the stainless steel oxidized iron balls produced from solid waste into the dephosphorized iron ladle through a high-level silo for smelting. Since the stainless steel oxidized iron balls contain more FeO, an oxidizing atmosphere can be provided for the iron ladle, thereby accelerating the dephosphorization reaction, increasing the dephosphorization rate, and reducing the smelting cost of low-phosphorus stainless steel.

[0015] 2. The implementation of this method has no impact on the original process of the dephosphorization station, is simple to operate, does not change the existing production model, and uses clay as a binder in the briquetting process, which has a low briquetting cost, saves energy and reduces emissions while improving the quality of steel products. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with embodiments: The diameter of the stainless steel iron oxide balls in the following embodiments of the present invention is 30-40 mm.

[0017] Example 1 The steel grade to be smelted this time is 430 ferritic stainless steel, and the smelting steps are as follows: This embodiment provides a method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls, comprising the following steps: (1) Preparing stainless steel iron oxide balls; using clay as a binder, pressing the stainless steel iron oxide into balls, the amount of clay used being 15wt% of the total weight of the stainless steel iron oxide balls, and drying naturally to obtain stainless steel iron oxide balls; the chemical composition of the stainless steel iron oxide balls is as follows in weight percentage: Si0 2 : 6.91%, Fe0: 50.1%, TFe: 63.5%, H 2 0:4%, the rest are uncontrollable elements brought from raw materials during carbon steel smelting; (2) transporting and loading materials; transporting the stainless steel iron oxide balls in step (1) to the third degassing warehouse, and lifting them to the silo by the bucket lifting belt for standby use; (3) Three-demetallization smelting process molten iron enters the station; blast furnace molten iron at a temperature of 1325°C is added to the pre-treated iron ladle, and the amount of molten iron added is 62.6 tons. The chemical composition of the molten iron is calculated by weight percentage: C: 4.59%, Si: 0.682%, Mn: 0.62%, P: 0.079%, and the rest is Fe and other uncontrollable elements brought from the raw materials; (4) Spray dephosphorization smelting; adding the stainless steel iron oxide balls in step (2) into the blast furnace molten iron in step (3), using nitrogen as a carrier gas to spray lime powder for deep dephosphorization and triple dephosphorization smelting; during the dephosphorization process, the spray pressure is 0.35 MPa, the lime powder injection amount is 30 kg / t molten iron, the amount of stainless steel iron oxide balls is 50 kg / t molten iron, and the feeding speed of the stainless steel iron oxide balls is 100 kg / min; ① Desiliconization period: In the early stage of smelting, oxygen is blown for desiliconization, and lime powder is sprayed to make slag. When the silicon content is reduced to 0.25%, the desiliconized slag is poured out; the oxygen flow rate of oxygen blowing for desiliconization during the desiliconization period is 38m 3 / min, lime powder injection flow rate is 42m 3 / min, nitrogen flow rate is 2.3m 3 / min, lime powder injection time is 11min, oxygen blowing volume is 460m 3 , the powder spraying amount is 462Kg, and 60% of the desiliconization slag is poured out after desiliconization; ② Secondary slagging and dephosphorization: After pouring out 60% of the desiliconized slag, continue to blow oxygen for desiliconization, and re-blow lime powder to make slag for dephosphorization; the oxygen flow rate during the secondary slagging and dephosphorization is 36m 3 / min, lime powder injection flow rate is 42m 3 / min, nitrogen flow rate is 2.3m 3 / min, dephosphorization alkalinity is 1.5, lime powder injection time is 27min, oxygen blowing volume is 1295m 3 , the powder spraying amount is 1418Kg, and the amount of stainless steel iron oxide balls is 1.8t; (5) Slag removal: After dephosphorization, 75% of the high-phosphorus slag produced in the ladle is removed by a slag remover. The slag removal time is 10 minutes. (6) Exit station: The measured C content in the molten iron is 3.54%, Si is 0.013%, Mn is 0.06%, and P is 0.009%, which meets the requirement of P ≤ 0.010% for low-phosphorus stainless steel. The molten iron is hoisted out of the dephosphorization station, and all high-phosphorus slag is removed before the molten iron leaves the station to prevent rephosphorization; (7) The molten iron after dephosphorization in step (6) is added into the AOD converter for decarburization and alloying operations.

[0018] By using the calculation method of (incoming phosphorus - outgoing phosphorus) / incoming phosphorus, it can be known that the dephosphorization rate during the smelting process of this embodiment is (0.079-0.009) / 0.079=88.6%.

[0019] Example 2 The steel grade to be smelted this time is J441 ultra-pure ferritic stainless steel, and the smelting steps are as follows: This embodiment provides a method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls, comprising the following steps: (1) Preparing stainless steel iron oxide balls; using clay as a binder, pressing the stainless steel iron oxide into balls, the amount of clay used is 12wt% of the total weight of the stainless steel iron oxide balls, and drying naturally to obtain stainless steel iron oxide balls; the chemical composition of the stainless steel iron oxide balls is as follows in weight percentage: Si0 2 : 6.91%, Fe0: 50.1%, TFe: 63.5%, H 2 0:4%, the rest are uncontrollable elements brought from raw materials during carbon steel smelting; (2) transporting and loading materials; transporting the stainless steel iron oxide balls in step (1) to the third degassing warehouse, and lifting them to the silo by the bucket belt for standby use; (3) Three-demetallization smelting process molten iron enters the station; blast furnace molten iron at a temperature of 1325°C is added to the pre-treated iron ladle, and the amount of molten iron added is 65.7 tons. The chemical composition of the molten iron is calculated by weight percentage: C: 4.39%, Si: 0.350%, Mn: 0.60%, P: 0.078%, and the rest is Fe and other uncontrollable elements brought from the raw materials; (4) Spray dephosphorization smelting; adding the stainless steel iron oxide balls in step (2) into the blast furnace molten iron in step (3), using nitrogen as a carrier gas to spray lime powder for deep dephosphorization and triple dephosphorization smelting; during the dephosphorization process, the spray pressure is 0.4 MPa, the amount of lime powder sprayed is 24 kg / t iron, the amount of stainless steel iron oxide balls used is 100 kg / t molten iron, and the feeding speed of the stainless steel iron oxide balls is 160 kg / min; ① Desiliconization period: In the early stage of smelting, oxygen is blown for desiliconization, and lime powder is sprayed to make slag. When the silicon content is reduced to 0.23%, the desiliconized slag is poured out; the oxygen flow rate during the desiliconization period is 40m 3 / min, lime powder injection flow rate is 42m 3 / min, nitrogen flow rate is 2.3m 3 / min, lime powder injection time is 15min, oxygen blowing volume is 600m 3 , the powder spraying amount is 625Kg, and 60% of the desiliconization slag is poured out after desiliconization; ② Secondary slagging and dephosphorization: After pouring out 60% of the desiliconized slag, continue to blow oxygen for desiliconization, and re-blow lime powder to make slag for dephosphorization; the oxygen flow rate during the secondary slagging and dephosphorization is 36m 3 / min, lime powder injection flow rate is 45m 3 / min, nitrogen flow rate is 2.5m 3 / min, dephosphorization alkalinity is 1.5, lime powder injection time is 30min, oxygen blowing volume is 1017m 3 , the powder spraying amount is 1055Kg, and the amount of stainless steel iron oxide balls is 2.8t; (5) Slag removal: After dephosphorization, 80% of the high-phosphorus slag produced in the ladle is removed by a slag remover. The slag removal time is 16 minutes. (6) Exit station: The measured C content in the molten iron is 3.25%, Si is 0.014%, Mn is 0.09%, and P is 0.007%, which meets the requirement of P ≤ 0.010% for low-phosphorus stainless steel. The molten iron is hoisted out of the dephosphorization station, and all high-phosphorus slag is removed before the molten iron leaves the station to prevent rephosphorization; (7) The molten iron after dephosphorization in step (6) is added into the AOD converter for decarburization and alloying operations.

[0020] By using the calculation method of (incoming phosphorus - outgoing phosphorus) / incoming phosphorus, it can be known that the dephosphorization rate during the smelting process of this embodiment is (0.078-0.007) / 0.078=91%.

[0021] Example 3 The steel grade to be smelted this time is J443 ultra-pure ferritic stainless steel, and the smelting steps are as follows: This embodiment provides a method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls, comprising the following steps: (1) Preparing stainless steel iron oxide balls; using clay as a binder, pressing the stainless steel iron oxide into balls, the amount of clay used is 10wt% of the total weight of the stainless steel iron oxide balls, and drying naturally to obtain stainless steel iron oxide balls; the chemical composition of the stainless steel iron oxide balls is as follows in weight percentage: Si0 2 : 6.91%, Fe0: 50.1%, TFe: 63.5%, H 20:4%, the rest are uncontrollable elements brought from raw materials during carbon steel smelting; (2) transporting and loading materials; transporting the stainless steel iron oxide balls in step (1) to the third degassing warehouse, and lifting them to the silo by the bucket lifting belt for standby use; (3) Three-demetallization smelting process molten iron enters the station; blast furnace molten iron at a temperature of 1320°C is added to the pre-treated iron ladle, and the amount of molten iron added is 61.3 tons. The chemical composition of the molten iron is calculated by weight percentage: C: 4.41%, Si: 0.471%, Mn: 0.56%, P: 0.084%, and the rest is Fe and other uncontrollable elements brought from the raw materials; (4) Spray dephosphorization smelting; adding the stainless steel iron oxide balls in step (2) into the blast furnace molten iron in step (3), using nitrogen as a carrier gas to spray lime powder for deep dephosphorization and triple dephosphorization smelting; during the dephosphorization process, the spray pressure is 0.35 MPa, the lime powder injection amount is 27 kg / t iron, the amount of stainless steel iron oxide balls is 80 kg / t iron, and the stainless steel iron oxide ball feeding speed is 140 kg / min; ① Desiliconization period: In the early stage of smelting, oxygen is blown for desiliconization, and lime powder is sprayed to make slag. When the silicon content is reduced to 0.25%, the desiliconized slag is poured out; the oxygen flow rate during the desiliconization period is 38m 3 / min, powder spraying flow rate is 40m 3 / min, the carrier gas flow rate is 2.3m 3 / min, the blowing time is 11min, and the oxygen blowing volume is 400m 3 , the powder spraying amount is 470Kg, and 60% of the desiliconization slag is poured out after desiliconization; ② Secondary slag dephosphorization: After pouring out 60% of the desiliconized slag, continue to blow oxygen for desiliconization, and re-blow lime powder to make slag for dephosphorization; the oxygen flow rate during the secondary slag dephosphorization is 30m 3 / min, powder spray flow rate is 35m 3 / min, the carrier gas flow rate is 2.3m 3 / min, dephosphorization alkalinity is 1.6, blowing time is 29min, oxygen blowing volume is 1020m 3 , the powder spraying amount is 1033Kg, and the amount of stainless steel iron oxide balls is 2.2t; (5) Slag removal: After dephosphorization, 75% of the high-phosphorus slag produced in the ladle is removed by a slag remover. The slag removal time is 8 minutes. (6) Exit station: The measured C content in the molten iron is 3.43%, Si is 0.018%, Mn is 0.19%, and P is 0.007%, which meets the requirement of P ≤ 0.010% for low-phosphorus stainless steel. The molten iron is hoisted out of the dephosphorization station, and all high-phosphorus slag is removed before the molten iron leaves the station to prevent rephosphorization; (7) The molten iron after dephosphorization in step (6) is added into the AOD converter for decarburization and alloying operations.

[0022] By using the calculation method of (incoming phosphorus - outgoing phosphorus) / incoming phosphorus, it can be known that the dephosphorization rate during the smelting process of this embodiment is (0.084-0.007) / 0.084=91.7%.

[0023] It can be seen from the above three embodiments that by adopting this method, the average dephosphorization rate reaches 90.4%, and the dephosphorization rate is greatly improved. The use of this method plays a significant role in controlling the phosphorus content of low-phosphorus stainless steel, and greatly improves the quality of steel products.

Claims

1. A method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls, characterized in that: The following steps are involved: (1) Preparing stainless steel iron oxide balls; using clay as a binder, pressing the stainless steel iron oxide into balls, and drying them naturally or in an oven to obtain stainless steel iron oxide balls; the chemical composition of the stainless steel iron oxide balls is, by weight percentage, 4%≤SiO2≤8%, Fe0≥45%, TFe≥55%, and H2O≤5%; (2) transporting and loading materials; transporting the stainless steel iron oxide balls in step (1) to the third degassing warehouse, and lifting them to the silo by the bucket belt for standby use; (3) The hot metal from the three-removal smelting process enters the station; the hot metal from the blast furnace is added to the pre-treated hot metal ladle. The chemical composition of the hot metal is calculated by weight percentage as follows: C ≥ 4.0%, Si: 0.3-1.0%, Mn ≤ 1.0%, P ≤ 0.1%, and the rest is Fe and other uncontrollable elements brought from the raw materials; (4) dephosphorization by spraying; adding the stainless steel iron oxide balls in step (2) into the molten iron in the blast furnace in step (3), and using nitrogen as a carrier gas to spray lime powder for deep dephosphorization and triple dephosphorization; ① Desiliconization period: In the early stage of smelting, oxygen is blown for desiliconization, and lime powder is sprayed to make slag. When the silicon content is reduced to <0.27%, the desiliconized slag is poured out; ② Secondary slagging and dephosphorization: After pouring out part of the desiliconized slag, continue to blow oxygen for desiliconization, and re-blow lime powder to make slag for dephosphorization; (5) Slag removal: After dephosphorization, the high-phosphorus slag produced in the ladle is removed by a slag remover to remove at least 70%; (6) Exit the station: After the P content in the molten iron is measured to be ≤ 0.010%, the molten iron is hoisted out of the dephosphorization station; (7) The molten iron after dephosphorization in step (6) is added to the AOD converter for decarburization and alloying operations.

2. The method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in claim 1, characterized in that: In step (1), the amount of clay used is 10-15wt% of the total weight of the stainless steel iron oxide ball.

3. The method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in claim 2, characterized in that: The diameter of the stainless steel iron oxide ball in step (1) is 30-40 mm.

4. A method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in claim 3, characterized in that: In step (3), the temperature of the molten iron in the blast furnace is 1280-1350°C.

5. A method for dephosphorizing and smelting low-phosphorus stainless steel in a hot metal ladle using stainless steel iron oxide balls as claimed in claim 4, characterized in that: In step (4), the amount of stainless steel iron oxide balls used is 50-100 kg / t molten iron, and the feeding speed of the stainless steel iron oxide balls is 80-160 kg / min.

6. A method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in any one of claims 1 to 5, characterized in that: In step (4), the amount of lime powder sprayed is 13-32 kg / t molten iron, and the spraying pressure is 0.30-0.40 MPa.

7. A method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in claim 6, characterized in that: Step (4) The oxygen flow rate of oxygen desiliconization during the desiliconization period is 36-40m 3 / min; lime powder injection flow rate is 40-45m 3 / min, nitrogen flow rate is 2.3-2.5m 3 / min, the lime powder injection time is 8-15min.

8. The method for smelting low-phosphorus stainless steel using stainless steel iron oxide balls as claimed in claim 7, characterized in that: The oxygen flow rate during the secondary slag dephosphorization in step (4) is 30-36m 3 / min; lime powder injection flow rate is 35-45m 3 / min, nitrogen flow rate is 2.3-2.5m 3 / min, dephosphorization alkalinity is 1.4-1.6, and lime powder injection time is 24-32min.