V-N microalloying and multi-stage heat treatment regulated high-toughness low-temperature maritime work steel and preparation method thereof

Through V-N microalloyation and multi-stage heat treatment technology, the problems of insufficient strength and high cost of existing marine engineering steels under low temperature conditions are solved, and low-cost low-temperature offshore engineering with high strength, low yield ratio and excellent low-temperature toughness are achieved. Steel reduces the use of Ni alloy and improves the comprehensive mechanical properties of steel.

CN119020699AActive Publication Date: 2024-11-26NORTHEASTERN UNIV CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411534249.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-26
Estimated Expiration
2044-10-31

AI Technical Summary

Technical Problem

The existing marine engineering steels are insufficient in strength, high yield and strength ratio, poor processing capacity under low temperature conditions, and high Ni alloy costs, resulting in increased smelting costs and insufficient material toughness.

Method used

Using V-N microalloyation and multi-stage heat treatment technology, nanoscale V(C,N) precipitates are formed by introducing V and N elements, combined with high-temperature quenching and sub-temperature quenching, the steel structure is optimized, and austenite stability is improved. Low temperature toughness.

Benefits of technology

Low-cost low-temperature offshore steel with high strength, low yield ratio and excellent low-temperature toughness is achieved, reducing the use of Ni alloys and improving the comprehensive mechanical properties and production efficiency of steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020699A_ABST
    Figure CN119020699A_ABST
Patent Text Reader

Abstract

The invention discloses V-N microalloying and multi-stage heat treatment regulated high-toughness low-temperature maritime work steel and a preparation method thereof, and belongs to the technical field of smelting of low-temperature alloy steel. V-N microalloying and multi-stage heat treatment are combined, the Ni content is reduced, V and N elements are added, meanwhile, the multi-stage heat treatment process of direct hot rolling quenching, high-temperature quenching, subcritical quenching and tempering is combined, resources are saved, meanwhile, the strength and low-temperature toughness of the material are improved, and therefore better strength and toughness matching is achieved; the low-temperature ocean engineering steel with good comprehensive performance is obtained, and guidance is provided for alloy design and process optimization of the high-performance ocean engineering steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of smelting steel for low-temperature alloys, and specifically relates to a high-strength and tough low-temperature marine engineering steel regulated by VN microalloying and multi-stage heat treatment, and a preparation method thereof. Background Art

[0002] With the development of my country's industry and the improvement of people's living standards, clean energy such as liquefied natural gas (LNG) and liquefied petroleum gas (LPG) are increasingly favored by people. However, due to the scarcity of domestic land oil (the main material for producing liquefied petroleum gas) and natural gas resources, their production is far from meeting the growing demand. The ocean is rich in oil and gas resources. At present, more than 80% of the world's marine oil and natural gas reserves are distributed in deep sea areas with a water depth of less than 500m, among which the oil and natural gas reserves in the Arctic region account for 13% and 30% of the world's undiscovered and unexploited reserves respectively. Therefore, it has become an inevitable trend for my country's oil and gas resource exploitation and transportation to move from land to deep sea and polar regions.

[0003] The development and transportation of deep-sea and polar resources cannot be separated from deep-diving-transportation technology, which is a comprehensive system composed of submersibles, surface support ships and land bases. Deep-sea surveys and assisting in the exploration and development of deep-sea resources all rely on submersibles. In order to cope with the complex marine environment, the steel used for submersibles should have high strength, excellent low-temperature toughness, good ductility and other characteristics to adapt to the static pressure and cyclically changing loads generated by the working depth during deep-sea operations. As a key engineering ship for polar scientific research, exploration and development, icebreakers need to continue icebreaking operations in the Arctic environment (air temperature below -50°C) and cooperate with submersibles for exploration. Due to the effect of sea ice, ships will be subject to additional ice loads during navigation in the Arctic. This long-term cyclic ice load is not only prone to damage to the hull structure components, but also places extremely high demands on the low-temperature toughness of the material. In addition, during the process of oil extraction, the offshore LPG production system will separate crude oil from LPG, and qualified LPG will be transported to storage tanks for storage. The natural gas obtained from mining is liquefied into LNG, which is smaller in volume and easier to store and transport. However, due to the ultra-low temperature and flammability of LPG and LNG, their transport tanks need to have excellent properties such as high strength, ultra-low temperature toughness and resistance to low-temperature crack growth.

[0004] At present, most of the marine engineering steels used in the market are low-alloy high-strength steels, mainly martensite, bainite or tempered martensite structures, and the austenite content in the steel is low. This results in a high yield strength ratio, insufficient processing capacity, difficulty in forming, and low service safety, although it has high strength. In addition, the thermal stability and mechanical stability of austenite in the structure are poor. Under low-temperature isothermal or low stress and strain conditions, martensitic phase transformation is prone to occur, transforming into brittle martensite, resulting in poor deep-cold toughness of the steel and unable to meet ultra-low service temperature conditions. In addition, in order to obtain a high-strength martensite / bainite matrix, traditional marine engineering steels usually use a higher carbon content, which will cause a large amount of cementite to precipitate, seriously deteriorate the low-temperature impact toughness and the ability to resist crack propagation, reduce the weldability of the steel plate, and pose a huge challenge to the manufacturing of hulls and high-end marine equipment and the safety of use under harsh conditions. Therefore, how to ensure high strength of marine engineering steel while retaining more stable austenite inside, reduce the yield ratio of steel, obtain good forming properties, improve its low-temperature toughness, and have excellent service safety at ultra-low temperatures is a current research hotspot.

[0005] The Ni element has the effect of improving the stability of austenite. Stable austenite can induce plasticity through local phase transformation, crack tip passivation and matrix purification, so that the steel has excellent impact toughness at a lower temperature. Therefore, Ni-based low-temperature marine steel can obtain good comprehensive mechanical properties and has broad research prospects in the fields of submersibles, icebreakers and cryogenic storage tanks. Among them, 9Ni steel is the most widely used because it can still maintain good low-temperature toughness at ultra-low temperatures. It can be used as a manufacturing material for equipment in service at -196℃ environment, such as the manufacture of LNG storage tanks. According to the EN 10028-4 standard, the performance requirements of traditional 9Ni steel are as follows: yield strength: 585MPa; tensile strength: 680MPa-820MPa; elongation: 18%; -196℃ impact energy: 80J.

[0006] In order to ensure high low-temperature toughness, a large amount of Ni alloy elements are added to traditional 9Ni steel to obtain a certain amount of metastable austenite. However, with the rapid development of science and technology, my country's demand for Ni alloys has increased, and a large amount of imports are required, which greatly increases the cost of steel smelting. At the same time, too high Ni content will lead to too high viscosity of molten steel, which is easy to cause continuous casting billet drawing failure after smelting, and in severe cases, it will cause steel leakage accidents. At the same time, although a high content of Ni elements has been added to 9Ni steel, there is still a problem of insufficient strength. The main reasons are as follows: On the one hand, in order to ensure low-temperature toughness, methods such as adding ultra-low carbon (≤0.05%) and removing impurity N are usually used to reduce the content of interstitial atoms (such as C, N, etc.) to prevent brittle fracture. On the other hand, 9Ni steel often ignores the addition of microalloying elements such as Nb, V, and Ti. Studies on related microalloyed steels have shown that adding 0.1% of microalloying elements to steel can obtain a strength increment of hundreds of MPa through the precipitation of nano-scale microalloying carbon and nitrides and the grain refinement caused by their pinning of grain boundaries. Therefore, due to the lack of C, N and micro-alloying elements in 9Ni steel, the effects of precipitation strengthening and fine grain strengthening cannot be fully exerted, and there is usually a problem of insufficient strength.

[0007] In addition to the influence of alloy composition on the mechanical properties of Ni-based low-temperature marine steel, heat treatment process is also a necessary way to regulate the mechanical properties of low-temperature marine steel. There are three common heat treatment processes for Ni-based low-temperature marine steel after hot rolling and air cooling: normalizing + tempering process, double normalizing + tempering process, and high-temperature quenching + tempering process. Among them, normalizing + tempering and double normalizing + tempering processes are rarely used in actual production because the obtained steel plate strength and low-temperature toughness are low and the energy consumption is high. High-temperature quenching + tempering is a method commonly used in industry at present. However, the content of metastable austenite obtained by high-temperature quenching + tempering process is low. Studies have shown that metastable austenite is often produced at grain boundaries, which can effectively prevent the generation and expansion of cracks and improve low-temperature toughness. Therefore, insufficient metastable austenite content will lead to poor crack propagation resistance of steel and cannot guarantee the low-temperature toughness of steel. At the same time, impurity atoms may be severely segregated at the grain boundaries, resulting in tempered martensite embrittlement, further reducing the impact toughness of steel. In addition, due to the poor enrichment effect of austenite stabilizing elements during high-temperature quenching + tempering, the stability of austenite is insufficient. In the low-temperature isothermal stage or under lower stress-strain conditions, unstable metastable austenite will be transformed into brittle martensite. The residual metastable austenite content is further reduced, the effect of inhibiting crack growth is weakened, and the low-temperature toughness is poor.

[0008] Therefore, there is an urgent need to develop a high-quality, high-strength and high-toughness low-temperature marine engineering steel. By optimizing the chemical composition of the steel and formulating a reasonable multi-stage heat treatment process, a nickel-saving low-temperature marine engineering steel that can meet the performance standards of 9Ni steel is developed. The purpose is to improve the mechanical properties of Ni-based low-temperature marine engineering steel, realize the production and development of low-cost, low-yield ratio, high strength, and excellent low-temperature toughness Ni-saving low-temperature marine engineering steel, and further promote the development of my country's shipbuilding and marine engineering industry. Summary of the invention

[0009] The purpose of the present invention is to provide a high-strength and tough low-temperature marine engineering steel and a method for preparing the same by VN microalloying and multi-stage heat treatment control, and to obtain a low-temperature marine engineering steel with good comprehensive performance by combining VN microalloying with multi-stage heat treatment, so as to provide guidance for the alloy design and process optimization of high-performance marine engineering steel.

[0010] To achieve the above object, the technical solution of the present invention is:

[0011] A VN microalloyed and multi-stage heat-treated high-strength and tough low-temperature marine engineering steel, the chemical composition weight percentage of which is: C 0.08%-0.15%, Ni 5.5%-7.5%, Mn 0.6%-1.5%, Mo 0.2%-0.84%, Si 0.2%-0.5%, V0.05%-0.3%, N 0.005%-0.014%, Al 0.02%-0.15%, S 0.002%-0.01%, P 0.002%-0.01%, and the balance is Fe and unavoidable impurities.

[0012] The microstructure of the low-temperature marine engineering steel after heat treatment includes tempered martensite, metastable austenite, fresh martensite and V (C, N) precipitates.

[0013] The low-temperature marine engineering steel has a thickness of 12 mm to 50 mm, a yield strength of 764 MPa to 925 MPa, a tensile strength of 840 MPa to 1040 MPa, a yield strength ratio of 0.88 to 0.91, an elongation of 20.2% to 25.6%, and an impact energy of 107 J to 152 J at -196°C.

[0014] The method for preparing the low-temperature high-strength and tough marine engineering steel by VN microalloying and multi-stage heat treatment regulation simulates the steps of industrial production: smelting, forging, hot rolling quenching, high-temperature quenching, sub-temperature quenching, and tempering. The specific steps are as follows:

[0015] Step 1. Smelting and forging:

[0016] In a vacuum induction furnace, an alloy ingot of the above composition is smelted and prepared, and the alloy ingot is heated to an austenitizing temperature range of 1140°C to 1220°C in a heating furnace, kept warm for 1h to 3.5h, and then forged into a steel billet in a temperature range of 980°C to 1220°C, with a thickness of 60mm to 150mm.

[0017] Step 2. Hot rolling and quenching treatment:

[0018] The forged steel billet is heated to 1140℃~1220℃, kept at this temperature for 1h~3.5h, and homogenized. Then, it is hot rolled, and after 5~7 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 12mm~50mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0019] Step 3. High temperature quenching treatment:

[0020] The hot-rolled steel plate after water quenching is heated to 800℃~830℃, kept at a temperature for 30min~60min after the temperature stabilizes, and then water quenched to room temperature.

[0021] Step 4. Sub-temperature quenching treatment:

[0022] The steel plate after high temperature quenching treatment is heated to the two-phase temperature of 650℃~690℃, kept warm for 40min~70min after the temperature stabilizes, and then water quenched to room temperature.

[0023] Step 5. Tempering:

[0024] The steel plate after sub-temperature quenching treatment is heated to 520°C~580°C, kept at a temperature for 60min~90min after the temperature stabilizes, and then air-cooled to room temperature to obtain a high-strength and tough low-temperature marine engineering steel regulated by VN microalloying and multi-stage heat treatment.

[0025] The marine engineering steel provided by the present invention is based on the traditional 9Ni low-temperature steel composition process, reducing the Ni element and adding V and N elements, while combining the hot rolling direct quenching-high temperature quenching-sub-temperature quenching-tempering multi-stage heat treatment process, while saving resources, improving the strength and low-temperature toughness of the material, thereby achieving better strength and toughness matching. On the one hand, V (C, N) precipitation phase is formed during the multi-stage heat treatment process, and the nano-scale V (C, N) precipitation phase will pin the grain boundary, accompanied by fine grain strengthening to obtain high strength. On the other hand, compared with the traditional heat treatment method, the cooling method after hot rolling is adjusted to direct quenching and the sub-temperature quenching process is added, which can better optimize the organization and performance of the steel. The direct water quenching method after hot rolling can greatly increase the cooling rate, increase the supercooling, increase the nucleation rate and increase the driving force of the phase change, thereby achieving the goal of grain refinement and helping to produce more stable austenite. Sub-temperature quenching is carried out in the two-phase region formed by austenite. This process can form metastable austenite with a high content, and austenite stabilizing elements such as Ni, Mn, C, and N in the alloy composition can be enriched in the metastable austenite, thereby improving the stability of the metastable austenite, so that it can still maintain a high content at ultra-low temperatures to hinder the expansion of cracks, and make the material have excellent low-temperature toughness. Under the condition of saving Ni and low cost, the present invention combines VN microalloying with a multi-stage heat treatment process, which not only avoids the problem of insufficient strength caused by the weak precipitation strengthening and fine grain strengthening capabilities under the original alloy system, but also overcomes the problem of low content and poor stability of metastable austenite under a single heat treatment process, so that the problem of difficulty in improving low-temperature toughness is solved. This innovative method helps to reduce production costs and improve product performance and competitiveness.

[0026] The present invention adopts low-carbon medium-nickel steel, adding a small amount of microalloying elements. C is an austenite stabilizing element, which can improve the strength of steel, but when the C content exceeds 0.2%, the low-temperature toughness of steel will be significantly reduced and the welding performance will be deteriorated, so the mass percentage of C is 0.08%~0.15%. Ni, as a key austenite stabilizing element, can significantly reduce the martensitic transformation temperature, so that metastable austenite can be kept at a high stability in a low-temperature environment, which is very beneficial to the improvement of the low-temperature toughness of steel. However, the Ni element is expensive. Under the premise of ensuring that the low-temperature mechanical properties of steel meet the requirements of use, it should be considered to carry out a quantitative treatment of the Ni element in the steel. Therefore, compared with the traditional 9Ni low-temperature marine steel, the mass percentage of Ni used in the present invention is 5.5%~7.5%. The Mn element is also an important austenite stabilizing element, which is conducive to the formation of reverse transformation austenite in steel, and can also reduce the martensitic transformation temperature in steel, which is very beneficial to improving the toughness of steel. The Mn element is also a matrix strengthening element, which has a certain solid solution strengthening effect on the matrix and can improve the hardenability of steel. Too low Mn content in steel will reduce the strength of steel and cannot meet the use requirements, while too high Mn content will lead to serious central segregation of steel billet, and will produce large-sized MnS inclusions, which will damage the toughness of steel. Therefore, the mass percentage of Mn used in the present invention is 0.6%~1.5%. Mo can stabilize austenite, avoid martensite temper brittleness, and improve low-temperature impact performance, but Mo is relatively expensive, so the mass percentage of Mo used in the present invention is 0.2%~0.84%. Si can be dissolved in austenite to produce solid solution strengthening, improve the hardness and strength of experimental steel, but when the silicon content exceeds a certain range, it will significantly reduce the plasticity and toughness of steel, so the mass percentage of Si used in the present invention is 0.2%~0.5%. my country has abundant V ore reserves, and the use of V solves the problem that other micro-alloy elements such as Nb have long relied on high-priced imports due to foreign monopoly. However, too much V addition will deteriorate the material processing performance and cause waste of resources. Therefore, the mass percentage of V used in the present invention is 0.05%~0.3%. N is an excellent austenite stabilizing element, and its ability to stabilize austenite is about 30 times that of Ni. In addition, N will combine with V to form VN microalloying, promote the precipitation of V (C, N), and improve strength, but too much N content will cause it to exist in the steel as interstitial atoms, significantly increase the brittleness of the steel, and damage the welding ability and cold bending performance of the steel. Therefore, the mass percentage of N used in the present invention is 0.005%~0.014%. Al is mainly used for deoxidation and grain refinement, and improves the toughness of steel at low temperatures, but excessive Al can cause Al to combine with N in large quantities to form AlN, resulting in hot brittleness of steel and easy cracking. Therefore, the mass percentage of Al used is 0.02%~0.15%. S and P are impurity elements in the test steel and should be controlled within a certain range.

[0027] The advantages of the present invention are:

[0028] (1) Optimize the alloy composition and introduce the concept of microalloying. The present invention proposes to introduce the concept of VN microalloying on the basis of ensuring a certain C content. On the one hand, V and N elements have a very strong affinity, which can regulate N not to exist in the form of interstitial atoms, and realize the precipitation of V (C, N) phase. This not only strengthens the precipitation strengthening effect, but also pins the original austenite and lath martensite grain boundaries, plays a role in refining grains and hindering dislocation movement, which can effectively improve the strength of the material. In addition, the fine grains can effectively hinder crack propagation and help improve toughness. On the other hand, a small amount of N will exist in the metastable austenite, which can improve the stability of the metastable austenite and contribute to the improvement of low-temperature toughness.

[0029] (2) Through multi-stage heat treatment, the organization and performance are regulated. On the basis of the traditional heat treatment process, water quenching is directly used instead of air cooling after hot rolling, which greatly improves the cooling rate, the nucleation rate is improved, and the grains are refined, which is conducive to obtaining fine lath martensite structure. Combined with the subsequent high temperature quenching (Q) process, cyclic quenching is formed, which further enhances the fine grain strengthening effect and contributes to the improvement of strength. These fine grains can also effectively prevent crack propagation and better improve the low temperature toughness of steel. In addition, the introduction of the sub-temperature quenching (L) process, some martensite rich in austenite stabilizing elements such as C, Mn, Ni, and N in the matrix will undergo a reverse transformation to form metastable austenite with a high content and uniform distribution, so that the matrix is ​​purified. The enrichment of alloying elements also improves the stability of metastable austenite. Finally, excellent impact toughness can be achieved at -196℃, providing performance support for practical applications.

[0030] (3) Multiple strengthening methods work together to improve strength. Compared with the traditional single optimization method, the combination of composition optimization and heat treatment process optimization adopted by the present invention can make the strength of steel far exceed the strength standard of 9Ni steel through multiple strengthening methods such as metal element solid solution strengthening, martensite lath strengthening, precipitation strengthening, fine grain strengthening, and work hardening, which plays a role in reducing structural weight, is conducive to reducing energy consumption and environmental pollution, and is of great significance for steel companies to upgrade marine engineering products and save energy and reduce consumption.

[0031] (4) Cost saving. my country has rich reserves of V ore, so the use of V solves the problem that other metals have long relied on high-priced imports due to foreign monopoly, thus reducing costs. N is a cheap element that is widely present in nature. Its cost is much lower than Ni and its ability to stabilize austenite is much higher than Ni. In addition, N and V have a high affinity, which can promote the precipitation of V (C, N), exert a more excellent precipitation strengthening and fine grain strengthening effect, and grain refinement helps to stabilize austenite. Recently, studies have shown that every 1% reduction in Ni in Ni-based low-temperature steel can reduce the cost by about 5%. Therefore, the present invention adds the N element to the steel, which has the effect of replacing Ni with N, can reduce the use of expensive Ni alloys, and greatly reduce the smelting cost of steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the heat treatment process of the present invention.

[0033] Figure 2 This is the SEM image of the tissue in Example 1.

[0034] Figure 3 This is the XRD diagram of Example 2.

[0035] Figure 4 This is the original austenite grain distribution diagram of Example 3.

[0036] Figure 5 This is the load / impact work-displacement curve of Example 4.

[0037] Figure 6 This is the impact fracture morphology of Example 5.

[0038] Figure 7 This is the SEM image of the tissue in Example 6.

[0039] Figure 8 This is the original austenite grain distribution diagram of the comparative example. DETAILED DESCRIPTION

[0040] The heating furnace used in the heat treatment process of the present invention is an atmosphere furnace produced by Siyang Precision Equipment (Shanghai) Co., Ltd.

[0041] The Japanese field emission scanning electron microscope JSM-7800F was used to observe the microstructure in the embodiment of the present invention.

[0042] The XRD test in the embodiment of the present invention adopts the Smart Lab 9kW of Japan Rigaku.

[0043] The tensile property test in the embodiment of the present invention is carried out using a Shimadzu tensile testing machine.

[0044] The impact performance test in the embodiment of the present invention adopts a PSW 750 Zwick pendulum impact tester.

[0045] The heat treatment process in the embodiment of the present invention is as follows Figure 1 shown.

[0046] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0047] Embodiment 1:

[0048] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.1%, Ni: 6.0%, Mn: 0.9%, Mo: 0.4%, Si: 0.25%, V: 0.2%, N: 0.007%, Al: 0.15%, S: 0.005%, P: 0.005%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1220℃, and the temperature is kept for 3h, and then forged into a steel billet with a thickness of 130mm in the temperature range of 1100℃~1220℃.

[0049] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1220℃, kept at this temperature for 3 hours, and homogenized. Then, hot rolling is performed. After 5 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 40mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0050] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 810°C, keep the temperature for 50 minutes after the temperature stabilizes, and then water quench to room temperature.

[0051] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 650°C, keep the temperature for 60 minutes after the temperature stabilizes, and then water quench to room temperature.

[0052] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 580°C, keep the temperature for 90 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0053] The prepared marine steel sample blank was ground into a mechanical property sample, and the performance test was carried out. The morphology analysis test was also carried out on it. The final microstructure SEM image obtained is as follows: Figure 2As shown in the figure, it can be seen that its structure is: tempered martensite + metastable austenite + fresh martensite + V (C, N) precipitates. Metastable austenite is dispersed on grain boundaries, intragranular and martensite lath boundaries. V (C, N) precipitates are spherical and evenly dispersed in the matrix. The mechanical properties of the prepared marine steel were tested, and its yield strength was 838MPa, tensile strength was 930MPa, yield strength ratio was 0.90, elongation was 21.5%, and impact energy at -196℃ was 115J.

[0054] Embodiment 2:

[0055] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.08%, Ni: 7.1%, Mn: 0.6%, Mo: 0.2%, Si: 0.5%, V: 0.05%, N: 0.005%, Al: 0.12%, S: 0.002%, P: 0.004%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1220℃, and the temperature is kept for 3.5h, and then forged into a steel billet with a thickness of 150mm in the temperature range of 1120℃~1220℃.

[0056] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1220°C, kept at this temperature for 3.5 hours, and homogenized. Then, hot rolling is performed. After 5 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 50 mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0057] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 830°C, keep the temperature for 60 minutes after the temperature stabilizes, and then water quench to room temperature.

[0058] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 690°C, keep the temperature for 70 minutes after the temperature stabilizes, and then water quench to room temperature.

[0059] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 540°C, keep the temperature for 90 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0060] The marine engineering steel sample prepared in this embodiment was subjected to XRD test to calculate the content of metastable austenite therein. The distribution of each substance peak is as follows: Figure 3As shown, according to the integrated intensity of austenite and martensite peaks, the content of metastable austenite in the marine engineering steel obtained in this embodiment is 14.2%. The obtained marine engineering steel sample blank is ground into a mechanical property sample and tested, and its mechanical properties are measured as follows: yield strength is 764MPa, tensile strength is 840MPa, yield strength ratio is 0.91, elongation is 20.2%, and impact energy at -196℃ is 107J.

[0061] Embodiment 3:

[0062] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.15%, Ni: 6.2%, Mn: 1.2%, Mo: 0.8%, Si: 0.2%, V: 0.3%, N: 0.014%, Al: 0.02%, S: 0.01%, P: 0.005%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1140℃, and the temperature is kept for 1h, and then forged into a steel billet with a thickness of 60mm in the temperature range of 980℃~1140℃.

[0063] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1140℃, kept at this temperature for 1 hour, and homogenized. Then, hot rolling is performed. After 7 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 12mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0064] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 800°C, keep the temperature for 30 minutes after the temperature stabilizes, and then water quench to room temperature.

[0065] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 660°C, keep the temperature for 40 minutes after the temperature stabilizes, and then water quench to room temperature.

[0066] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 550°C, keep the temperature for 60 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0067] The morphology of the marine engineering steel prepared in this embodiment was tested, and the original austenite grain distribution was as follows: Figure 4As shown. The original austenite grain size is statistically analyzed, and its grain size is relatively small, with an average size of 15.41μm, and the grain size distribution is relatively uniform. Such fine and uniform grains help to improve the mechanical properties of the material. The prepared marine steel sample blank was ground into a mechanical property sample for testing, and its mechanical properties were measured as follows: yield strength of 925MPa, tensile strength of 1040MPa, yield strength ratio of 0.89, elongation of 22.4%, and impact energy of 132J at -196℃.

[0068] Embodiment 4:

[0069] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.12%, Ni: 5.5%, Mn: 1.0%, Mo: 0.62%, Si: 0.32%, V: 0.2%, N: 0.012%, Al: 0.04%, S: 0.006%, P: 0.01%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1200℃, and the temperature is kept for 2.5h, and then forged into a steel billet with a thickness of 120mm in the temperature range of 1060℃~1200℃.

[0070] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1180°C, kept warm for 3 hours, homogenized, and then hot rolled. After 6 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 30 mm. Finally, the hot-rolled steel plate is directly water quenched to room temperature.

[0071] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 810°C, keep the temperature for 45 minutes after the temperature stabilizes, and then water quench to room temperature.

[0072] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 660°C, keep the temperature for 60 minutes after the temperature stabilizes, and then water quench to room temperature.

[0073] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 560°C, keep the temperature for 80 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0074] The marine steel sample blank prepared in this embodiment was ground into a mechanical property sample and tested. The mechanical properties were measured as follows: yield strength of 865MPa, tensile strength of 960MPa, yield strength ratio of 0.90, elongation of 21.8%, and impact energy of 119J at -196℃. The load / impact energy-displacement curve obtained during the low-temperature impact process at -196℃ is shown in FIG. Figure 5As shown in the figure, according to the load / impact work-displacement curve, the energy corresponding to the impact from the beginning to the maximum value of the impact load is the crack formation work, which is 41J. The energy corresponding to the process from the maximum load to the occurrence of fracture is the crack extension work: 78J. The sum of the two is the total impact work of 119J.

[0075] Embodiment 5:

[0076] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.1%, Ni: 7.5%, Mn: 0.9%, Mo: 0.84%, Si: 0.43%, V: 0.12%, N: 0.009%, Al: 0.09%, S: 0.008%, P: 0.007%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1150℃, and the temperature is kept for 2h, and then forged into a steel billet with a thickness of 90mm in the temperature range of 1000℃~1150℃.

[0077] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1150℃, kept at this temperature for 2 hours, and homogenized. Then, hot rolling is performed. After 7 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 17mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0078] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 810°C, keep the temperature for 35 minutes after the temperature stabilizes, and then water quench to room temperature.

[0079] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 690°C, keep the temperature for 45 minutes after the temperature stabilizes, and then water quench to room temperature.

[0080] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 570°C, keep the temperature for 65 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0081] The marine steel sample blank prepared in this embodiment was ground into a mechanical property sample and tested. The mechanical properties were measured as follows: yield strength of 841 MPa, tensile strength of 955 MPa, yield strength ratio of 0.88, elongation of 25.6%, and impact energy of 152 J at -196°C. The micro-fracture morphology of the sample after impact at -196°C (such as Figure 6 After observation (as shown in the figure), it was found that the fracture of the impact specimen produced significant plastic deformation, consisting of a large dimple and surrounding small equiaxed dimples, showing ductile fracture characteristics, indicating that the deep cold impact toughness is good.

[0082] Embodiment 6:

[0083] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingot is as follows in mass percentage: C: 0.13%, Ni: 6.7%, Mn: 1.5%, Mo: 0.7%, Si: 0.35%, V: 0.3%, N: 0.01%, Al: 0.06%, S: 0.004%, P: 0.002%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1200℃, and the temperature is kept for 2h, and then forged into a steel billet with a thickness of 100mm in the temperature range of 1050℃~1200℃.

[0084] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1180℃, kept at this temperature for 2 hours, and homogenized. Then, hot rolling is performed. After 6 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 25mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0085] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 800°C, keep the temperature for 40 minutes after the temperature stabilizes, and then water quench to room temperature.

[0086] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 670°C, keep the temperature for 50 minutes after the temperature stabilizes, and then water quench to room temperature.

[0087] Step 5. Tempering treatment: heat the steel plate after sub-temperature quenching treatment to 520°C, keep the temperature for 70 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain high-strength and toughness low-temperature marine engineering steel with VN micro-alloying and multi-stage heat treatment control.

[0088] The morphology of the marine steel structure obtained in this embodiment was analyzed, and the final structure SEM image obtained was as follows: Figure 7 As shown, the structure is the same as other embodiments: the matrix is ​​a tempered martensite structure, and the bright lining area on the matrix is ​​mainly metastable austenite and fresh martensite generated during the cooling process, and V (C, N) precipitates are formed at the same time. Among them, the metastable austenite is in the form of relatively small, discontinuous dots, dispersed on the grain boundaries, in the grains and on the martensite lath boundaries; while the fresh martensite is distributed in a relatively scattered and coarse manner. The V (C, N) precipitates are spherical, relatively small in size, and evenly dispersed in the matrix. At the same time, the marine steel sample blank prepared in this embodiment was ground into a mechanical property sample, and the mechanical property test was carried out on it. The mechanical properties are as follows: the yield strength is 890MPa, the tensile strength is 1000MPa, the yield strength ratio is 0.89, the elongation is 23.5%, and the impact energy at -196°C is 137J.

[0089] Comparative Example:

[0090] Step 1. Smelting and forging: Smelt and prepare alloy ingots in a vacuum induction furnace. The composition of the alloy ingots is as follows in mass percentage: C: 0.08%, Ni: 7.2%, Mn: 0.72%, Mo: 0.35%, Si: 0.23%, Al: 0.07%, S: 0.003%, P: 0.003%, and the remaining content is Fe and unavoidable impurities. The alloy ingot is heated to the austenitizing temperature in a heating furnace, the heating temperature is controlled at 1220℃, and the temperature is kept for 3.5h, and then forged into a steel billet with a thickness of 150mm in the temperature range of 1120℃~1220℃.

[0091] Step 2. Hot rolling quenching treatment: The forged steel billet is heated to 1220°C, kept at this temperature for 3.5 hours, and homogenized. Then, hot rolling is performed. After 5 rolling processes, the steel billet is rolled into a hot-rolled steel plate with a thickness of 50 mm, and finally the hot-rolled steel plate is directly water quenched to room temperature.

[0092] Step 3. High temperature quenching treatment: heat the hot-rolled steel plate after water quenching to 820°C, keep the temperature for 60 minutes after the temperature stabilizes, and then water quench to room temperature.

[0093] Step 4. Sub-temperature quenching treatment: Heat the steel plate after high-temperature quenching treatment to the two-phase temperature of 680°C, keep the temperature for 70 minutes after the temperature stabilizes, and then water quench to room temperature.

[0094] Step 5. Tempering treatment: Heat the steel plate after sub-temperature quenching treatment to 580°C, keep the temperature for 90 minutes after the temperature stabilizes, and then air-cool to room temperature to obtain the marine steel product.

[0095] After the comparative sample was corroded with picric acid, the original austenite grain distribution diagram was obtained as shown in the figure below. Figure 8 As shown. The original austenite grain size was statistically analyzed and found to be relatively coarse, with an average size of 22.14 μm. In addition, the grain size distribution is uneven, with the difference between the largest grain and the smallest grain size being approximately 13 μm, which is a large difference. At the same time, the marine steel sample blank obtained in this comparative example was ground into a mechanical property sample, and the corresponding performance tests were carried out. The mechanical properties were measured to be: yield strength of 748 MPa, tensile strength of 797 MPa, yield strength ratio of 0.94, elongation of 16.4%, and impact energy of 75 J at -196 °C.

[0096] In summary, by comparing the examples with the comparative examples, it is found that the introduction of the concept of VN microalloying in steel and the combination with multi-stage heat treatment can make more nano-scale V(C,N) precipitates precipitate in low-temperature marine engineering steel, and the structure becomes finer, which has a more obvious pinning effect on dislocations and significantly improves the strength. In addition, a certain amount of stable metastable austenite will be obtained during the heat treatment process, so that it still has better low-temperature impact toughness than the comparative example at a low temperature of -196°C, which is conducive to the formation of excellent strength and toughness matching, and has made certain contributions to the development of low-temperature marine engineering steel.

Claims

1. A high-strength and low-temperature marine engineering steel with VN microalloying and multi-stage heat treatment control, characterized in that: The chemical composition mass percentage of the marine steel is: C 0.08%~0.15%, Ni 5.5%~7.5%, Mn 0.6%~1.5%, Mo 0.2%~0.84%, Si0.2%~0.5%, V 0.05%~0.3%, N 0.005%~0.014%, Al 0.02%~0.15%, S 0.002%~0.01%, P 0.002%~0.01%, and the balance is Fe and unavoidable impurities; The microstructure of the low-temperature marine engineering steel after heat treatment includes tempered martensite, metastable austenite, fresh martensite and V (C, N) precipitates.

2. The high-strength and low-temperature marine engineering steel with VN microalloying and multi-stage heat treatment control according to claim 1, characterized in that: The low-temperature marine engineering steel has a thickness of 12 mm to 50 mm, a yield strength of 764 MPa to 925 MPa, a tensile strength of 840 MPa to 1040 MPa, a yield strength ratio of 0.88 to 0.91, an elongation of 20.2% to 25.6%, and an impact energy of 107 J to 152 J at -196°C.

3. The method for preparing the high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 1 or 2, characterized in that: The steps of simulating industrial production: smelting, forging, hot rolling quenching, high temperature quenching, sub-temperature quenching, tempering, the specific steps are as follows: Step 1. Smelting and forging: Smelting an alloy ingot containing the marine steel component in a vacuum induction furnace, heating and keeping the alloy ingot warm, and then forging it into a steel billet at a temperature ranging from 980° C. to 1220° C.; Step 2. Hot rolling and quenching treatment: The forged steel billet is heated, kept warm, homogenized, and then hot rolled to obtain a hot-rolled steel plate, and then the hot-rolled steel plate is directly water quenched to room temperature; wherein the hot rolling passes are 5 to 7; Step 3. High temperature quenching treatment: The hot-rolled steel plate after water quenching is heated to 800°C~830°C, kept at a stable temperature, and then water quenched to room temperature; Step 4. Sub-temperature quenching treatment: The high-temperature quenched steel plate is heated to a two-phase temperature of 650°C to 690°C, kept warm after the temperature stabilizes, and then water quenched to room temperature; Step 5. Tempering: The steel plate after the sub-temperature quenching treatment is heated to 520°C~580°C, kept warm after the temperature stabilizes, and then air-cooled to room temperature to obtain a high-strength and tough low-temperature marine steel regulated by VN microalloying and multi-stage heat treatment.

4. The method for preparing high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 3, characterized in that: In step 1, the alloy ingot is heated to a temperature of 1140°C to 1220°C, and the holding time is 1h to 3.5h; The thickness of the steel billet is 60 mm to 150 mm.

5. The method for preparing high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 3, characterized in that: In step 2, the heating temperature of the steel billet is 1140°C to 1220°C, and the holding time is 1h to 3.5h; The thickness of the hot-rolled steel plate is 12 mm to 50 mm.

6. The method for preparing high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 3, characterized in that: In step 3, the insulation time is 30 min to 60 min.

7. The method for preparing high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 3, characterized in that: In step 4, the insulation time is 40 min to 70 min.

8. The method for preparing high-strength and low-temperature marine engineering steel by VN microalloying and multi-stage heat treatment control according to claim 3, characterized in that: In step 5, the insulation time is 60 min to 90 min.

Citation Information

Patent Citations

  • Method for manufacturing low-carbon 9Ni steel thick plate

    CN101215668A

  • Manufacturing method of steel with high-strength and high-toughness for ocean engineering

    CN113355583A

  • 1000MPa-grade structural steel and preparation method thereof

    CN118406971A

  • Gigabit-grade maritime work steel plate used in extremely cold and ultra-deep environment and manufacturing method of gigabit-grade maritime work steel plate

    CN118639141A

  • A 9ni steel plate for ship LNG storage tank with high strength and low yield ratio and its production method

    US20230323494A1