Hot-rolled wire rod for high-strength steel wire rope and preparation method of hot-rolled wire rod

Hot-rolled strips for high-strength wire ropes are prepared through high-strength wire rolling and controlled rolling and cold-controlled processes, which solves the problems of high alloy addition and heat treatment costs in the prior art, and achieves high-strength and good torsion and bending performance of wire ropes.

CN118996084AActive Publication Date: 2024-11-22PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP +1

Patent Information

Application Number
CN202411216068.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

During the production process of existing high-strength wire ropes, the addition of alloy increases production costs and easily leads to reduced plasticity. The heat treatment is complex and costly, making it difficult to meet the needs of high strength and good torsion and bending performance.

Method used

Using high-line rolling and controlled rolling and cooling processes, hot-rolling strips for high-strength wire ropes are prepared through the heating temperature, heating time, wire spinning temperature after rolling and sectional cooling technology to ensure nominal tensile strength ≥1870MPa, twisting times ≥25 times, bending times ≥15 times.

Benefits of technology

The production of high-strength wire ropes has been realized, which reduces production costs, improves the performance of wire ropes, and meets the market's requirements for high-strength and multiple twisting and bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996084A_ABST
    Figure CN118996084A_ABST
Patent Text Reader

Abstract

The invention discloses a hot-rolled wire rod for a high-strength steel wire rope and a preparation method of the hot-rolled wire rod. The method comprises the following steps: smelting in a converter, refining outside the converter and continuously casting to obtain a required casting blank; and then casting blank heating, high-pressure water dephosphorization, high-speed wire rolling, silking of a silking machine, stelmor air cooling line controlled cooling, coiling and packaging are conducted in sequence, and the hot-rolled wire rod for the high-strength steel wire rope is obtained. Wherein in the rolling process, the multiple water tanks are divided into multiple groups, and the opening degrees, the outlet pressure and the flow of the multiple groups of water tanks are gradually reduced in the direction of a rolling production line; in the stelmor air cooling line controlled cooling process, the multiple draught fans are divided into multiple sets, and the opening degrees of the multiple sets of draught fans are gradually reduced in the stelmor air cooling line direction. The method mainly comprises a high-speed wire rolling procedure and a controlled rolling and controlled cooling procedure, and a hot-rolled wire rod with good performance is finally obtained by combining control of casting blank heating temperature, heating time and spinning temperature after rolling and a segmented controlled cooling technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a hot-rolled wire rod for high-strength steel wire rope and a preparation method thereof. Background Art

[0002] Steel wire ropes are widely used in many fields such as elevator hoisting, automobile lifting, port loading and unloading, and mine hoisting. At present, ordinary steel wire ropes below 1770MPa are widely used. With the continuous development of my country's machinery industry, the market demand for high-strength steel wire ropes of 1870MPa and above is increasing.

[0003] High-strength steel wire ropes are not only required to have high nominal tensile strength, but also have high requirements for torsion and bending properties, so as to ensure their safety and long service life. This also puts forward new requirements for the wire rods used to make steel wire ropes. In order to improve the strength of the wire rods, alloys are usually added or heat treated. However, the addition of alloys not only increases the production cost, but also easily leads to reduced plasticity, resulting in brittle fracture during the drawing and twisting process of the steel wire rope. Heat treatment will complicate the production process of the steel wire rope and further increase the production cost of the steel wire rope.

[0004] In view of this, the existing technology should be improved. Summary of the invention

[0005] The main purpose of the present invention is to provide a hot-rolled wire rod for high-strength steel wire rope and a preparation method thereof, which mainly includes high-wire rolling and controlled rolling and controlled cooling processes. By combining the heating temperature, heating time, and wire-laying temperature of the ingot casting with the control of the segmented controlled cooling technology, a hot-rolled wire rod with good performance is finally obtained. The hot-rolled wire rod can be used to make a high-strength steel wire rope with a nominal tensile strength of ≥1870MPa, a torsion number of ≥25 times, and a bending number of ≥15 times.

[0006] According to one aspect of the present invention, a method for preparing a hot-rolled wire rod for high-strength steel wire rope is proposed, which comprises: sequentially performing converter smelting, refining outside the furnace, and continuous casting to obtain the desired ingot, and then sequentially performing ingot heating, high-pressure water dephosphorization, high-wire rolling, spinning on a spinning machine, controlled cooling on a Stelmore air-cooling line, coiling and packaging to obtain the hot-rolled wire rod for high-strength steel wire rope; wherein, during the rolling process, a plurality of water tanks are divided into a plurality of groups, and along the direction of the rolling production line, the opening degree, outlet pressure and flow rate of the plurality of water tanks are gradually reduced; during the controlled cooling process of the Stelmore air-cooling line, a plurality of fans are divided into a plurality of groups, and along the direction of the Stelmore air-cooling line, the opening degree of the plurality of fans is gradually reduced.

[0007] According to one embodiment of the present invention, the chemical composition of the hot-rolled wire rod for high-strength steel wire rope is as follows in weight percentage: C: 0.60% to 0.70%, Si: 0.40% to 0.80%, Mn: 0.30% to 0.60%, P≤0.015%, S≤0.010%, Cr: 0.10% to 0.30%; the rest is Fe and unavoidable impurities.

[0008] According to one embodiment of the present invention, during the continuous casting process, the superheat degree of the molten steel is 10-25° C., the casting speed is constant, and the central carbon segregation degree of the ingot is 0.98-1.06.

[0009] According to one embodiment of the present invention, the heating of the ingot is performed by a heating furnace, the temperature range of the soaking section of the heating furnace is 1000-1050°C, and the heating time t=(0.8-1.2)H, wherein H is the thickness of the ingot.

[0010] According to one embodiment of the present invention, the ingot is heated in a heating furnace, dephosphorized by high-pressure water, and then rolled into a wire rod on a high-speed wire. The rolling temperature is 920-980°C, and the rolling process is controlled by cooling water.

[0011] According to one embodiment of the present invention, during the rolling process, the opening degree of the 1# water tank is 20-30%, the outlet water pressure is 3-4 bar, and the flow rate is 20-30 m 3 / h, the opening degree of 2# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 3# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 4# water tank is 15~25%, the outlet water pressure is 1.5~2.5bar, and the flow rate is 15~20m 3 / h, 5# water tank opening degree ≤10%, outlet water pressure ≤1.5bar, flow rate ≤10m 3 / h, the temperature before spinning is 850~885℃.

[0012] According to one embodiment of the present invention, the wire rod after spinning is controlled to be cooled in a Stelmore air cooling line, the initial roller speed is 0.6-0.7 m / s, and the speed of the 2nd to 13th roller sections is increased by 0.01-0.03 m / s.

[0013] According to one embodiment of the present invention, in the Stelmore air cooling line, the opening degree of 1# to 5# fans is 95~100%, the opening degree of 6# fan is 75~85%, the opening degree of 7# fan is 65~75%, the opening degree of 8# fan is 55~65%, the thermal insulation covers are all opened, and the opening angle of the Jialing device is 3~8°; when rapidly cooled to 600~630℃, the fans and thermal insulation covers are turned off, and slow cooling is carried out at a cooling rate of ≤3℃ / s, and the coiling temperature is ≤450℃.

[0014] According to another aspect of the present invention, a hot-rolled wire rod for high-strength steel wire rope is provided, which is prepared by any of the methods in the above technical solutions.

[0015] According to one embodiment of the present invention, the hot-rolled wire rod for high-strength steel wire rope has a tensile strength of ≥1200MPa, an elongation after fracture ≥15%, a cross-sectional shrinkage rate ≥45%, a structure of pearlite + trace ferrite, a troostite rate ≥85%, and no central martensite and grain boundary cementite.

[0016] In a preparation method of a hot-rolled wire rod for high-strength steel wire rope according to an embodiment of the present invention, it mainly includes high-wire rolling and controlled rolling and controlled cooling processes. By combining the control of the heating temperature, heating time, and wire-laying temperature after rolling as well as the segmented controlled cooling technology, a hot-rolled wire rod with good performance is finally obtained. The hot-rolled wire rod can be used to make a high-strength steel wire rope with a nominal tensile strength ≥1870MPa, a torsion number ≥25 times, and a bending number ≥15 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A process flow chart of a method for preparing a hot-rolled wire rod for a high-strength steel wire rope according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION

[0019] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0020] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0021] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0022] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0023] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0024] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.

[0025] like Figure 1As shown, the present invention provides a method for preparing a hot-rolled wire rod for high-strength steel wire rope, which comprises the following steps: S1, sequentially performing converter smelting, refining outside the furnace, and continuous casting to obtain the desired ingot; S2, sequentially performing ingot heating, high-pressure water dephosphorization, high-wire rolling, wire laying on a laying machine, controlled cooling on a Stelmore air-cooling line, coiling and packaging to obtain the hot-rolled wire rod for high-strength steel wire rope; wherein, during the rolling process, a plurality of water tanks are divided into a plurality of groups, and along the direction of the rolling production line, the opening degree, outlet pressure and flow rate of the plurality of water tanks are gradually reduced; during the controlled cooling process of the Stelmore air-cooling line, a plurality of fans are divided into a plurality of groups, and along the direction of the Stelmore air-cooling line, the opening degree of the plurality of fans is gradually reduced.

[0026] In the preparation method of the hot-rolled wire rod for high-strength steel wire rope according to the embodiment of the present invention, it mainly includes high-wire rolling and controlled rolling and controlled cooling processes. By combining the control of the heating temperature, heating time, and wire-spinning temperature after rolling as well as the segmented controlled cooling technology, a hot-rolled wire rod with good performance is finally obtained. The hot-rolled wire rod can be used to make a high-strength steel wire rope with a nominal tensile strength ≥1870MPa, a torsion number ≥25 times, and a bending number ≥15 times.

[0027] In some specific embodiments, the chemical composition of the hot-rolled wire rod for high-strength steel wire rope is as follows by weight percentage: C: 0.60% to 0.70%, Si: 0.40% to 0.80%, Mn: 0.30% to 0.60%, P≤0.015%, S≤0.010%, Cr: 0.10% to 0.30%; the rest is Fe and unavoidable impurities.

[0028] On the basis of the above embodiments, during the continuous casting process, the superheat of the molten steel is 10-25°C, the casting speed is constant, and the central carbon segregation of the ingot is 0.98-1.06.

[0029] The superheat of molten steel is an important factor affecting the center segregation of the ingot. Excessive superheat will intensify the growth of columnar crystals, promote the enrichment of solute elements, and thus increase the center segregation. Therefore, setting a reasonable tundish superheat, such as stabilizing it below 20°C, or even below 15°C, can effectively reduce the center carbon segregation of the ingot and improve the internal quality of the ingot.

[0030] Constant casting speed can ensure that the billet is cooled and compensated evenly and stably during solidification, thus avoiding the problem of unstable internal quality of the billet caused by fluctuations in casting speed. Constant casting speed helps to reduce defects such as cracks and looseness inside the billet and improve the overall quality of the billet.

[0031] In some specific embodiments, the heating of the ingot is performed by a heating furnace, the temperature range of the soaking section of the heating furnace is 1000-1050° C., and the heating time t=(0.8-1.2)H, wherein H is the thickness of the ingot.

[0032] On the basis of the above embodiment, the billet is heated in a heating furnace, and then dephosphorized by high-pressure water and rolled into a wire rod on a high-speed wire. The rolling temperature is 920-980°C, and the rolling process is controlled by cooling water. Specifically, the billet is dephosphorized by high-pressure water and rolled into a φ6.5mm wire rod on a high-speed wire.

[0033] In some specific embodiments, during the rolling process, the opening degree of the 1# water tank is 20-30%, the outlet water pressure is 3-4 bar, and the flow rate is 20-30 m 3 / h, the opening degree of 2# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 3# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 4# water tank is 15~25%, the outlet water pressure is 1.5~2.5bar, and the flow rate is 15~20m 3 / h, 5# water tank opening degree ≤10%, outlet water pressure ≤1.5bar, flow rate ≤10m 3 / h, the temperature before spinning is 850~885℃. 1#~5# water tanks are arranged in sequence along the rolling production line.

[0034] Specifically, the opening degree of the 1# water tank is 25%, the outlet water pressure is 3.5 bar, and the flow rate is 25m 3 / h, the opening degree of 2# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 3# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 4# water tank is 20%, the outlet water pressure is 2.0 bar, and the flow rate is 18m 3 / h, 5# water tank opening degree ≤10%, outlet water pressure ≤1.5bar, flow rate ≤10m 3 / h, the temperature before spinning is 850~885℃.

[0035] On the basis of the above embodiments, the wire rod after spinning is controlled cooled in the Stelmore air cooling line, the initial roller speed is 0.6-0.7 m / s, and the speed of the 2nd to 13th rollers is increased by 0.01-0.03 m / s.

[0036] Specifically, the initial roller speed is 0.68 m / s, and the roller speeds of the 2nd to 13th sections increase by 0.02 m / s step by step.

[0037] In some specific embodiments, in the Stelmore air cooling line, the opening degree of 1#~5# fans is 95~100%, the opening degree of 6# fan is 75~85%, the opening degree of 7# fan is 65~75%, the opening degree of 8# fan is 55~65%, the insulation covers are all opened, and the opening angle of the Jialing device is 3~8°; when rapidly cooled to 600~630℃, the fans and insulation covers are turned off, and slow cooling is performed at a cooling rate of ≤3℃ / s, and the coiling temperature is ≤450℃. 1#~7# fans are arranged in sequence along the direction of the Stelmore air cooling line. The flow rate of 1#~4# fans is 190,000~210,000m 3 / h, the flow rate of 5# fan is 150,000-170,000 m 3 / h, the flow rate of 6# fan is 120,000-130,000 m 3 / h, the flow rate of 7# fan is 110,000-120,000 m 3 / h, the flow rate of 8# fan is 90,000-100,000 m 3 / h.

[0038] Specifically, the opening degree of 1#~5# fans is 100%, the opening degree of 6# fan is 80%, the opening degree of 7# fan is 70%, the opening degree of 8# fan is 60%, the insulation covers are all opened, and the opening angle of the Jialing device is 5°; when rapidly cooled to 600~630℃, the fans and insulation covers are turned off, and slow cooling is carried out at a cooling rate of ≤3℃ / s, and the coiling temperature is ≤450℃.

[0039] The present invention also proposes a hot-rolled wire rod for high-strength steel wire rope, which is prepared by the method mentioned in the above technical solution.

[0040] In some specific embodiments, the hot-rolled wire rod for high-strength steel wire rope has a tensile strength of ≥1200 MPa, an elongation after fracture of ≥15%, a cross-sectional shrinkage of ≥45%, a structure of pearlite + trace ferrite, a troostite rate of ≥85%, and no central martensite and grain boundary cementite.

[0041] The steel wire rope made from this wire rod has a nominal tensile strength ≥1870MPa, a torsion number ≥25 times, and a bending number ≥15 times.

[0042] A specific application of the present invention is: The first step: through converter smelting, refining outside the furnace, and continuous casting, the required ingot with chemical composition meeting the requirements is obtained.

[0043] (1) During the continuous casting process of the ingot preparation, the superheat of the molten steel is 10-25°C, the casting speed is constant, and the central carbon segregation of the ingot is 0.98-1.06.

[0044] (2) Chemical composition of the ingot: C 0.60%~0.70%, Si 0.40%~0.80%, Mn 0.30%~0.60%, P≤0.015%, S≤0.010%, Cr 0.10%~0.30%; the rest are Fe and unavoidable impurities.

[0045] Step 2: Heat the obtained ingot through a heating furnace. The temperature of the heating furnace soaking section is 1000-1050°C. The heating time is t= (0.8-1.2)H, where H is the thickness of the ingot.

[0046] Step 3: After heating in a heating furnace, the ingot is cast and then dephosphorized by high-pressure water and rolled into φ6.5mm wire rod on a high-speed wire.

[0047] (1) The rolling temperature is 920-980°C.

[0048] (2) During the rolling process, the water cooling box is turned on for water cooling to reduce the temperature of the rolled piece and ensure that the wire drawing temperature is controlled within the required range. The opening degree of the 1# water tank is 25%, the outlet water pressure is 3.5 bar, and the flow rate is 25m 3 / h, the opening degree of 2# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 3# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 4# water tank is 20%, the outlet water pressure is 2.0 bar, and the flow rate is 18m 3 / h, 5# water tank opening degree ≤10%, outlet water pressure ≤1.5bar, flow rate ≤10m 3 / h, the spinning temperature is 850~885℃.

[0049] (3) The wire rod after spinning is controlled to be cooled in the Stelmor air cooling line. The initial roller speed is 0.68m / s, and the roller speed of the 2nd to 13th sections increases by 0.02m / s; the opening degree of 1# to 4# fans is 100%, and the flow rate is 200,000m 3 / h, the corresponding insulation cover is open; the opening degree of 5# fan is 100%, and the flow rate is 160,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 6# fan is 80%, and the flow rate is 128,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 7# fan is 70%, and the flow rate is 112,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 8# fan is 60%, and the flow rate is 96,000 m 3 / h, the corresponding insulation cover is opened; the opening angle of the Jialing device is 5°; when the temperature is quickly cooled to 600-630℃, the fan and the corresponding insulation cover are turned off, and slow cooling is carried out at a cooling rate of ≤3℃ / s, and the coiling temperature is ≤450℃.

[0050] The present invention also provides a hot-rolled wire rod for high-strength steel wire rope, which is prepared by any method of the above technical solutions.

[0051] The hot-rolled wire rod for high-strength steel wire rope has a tensile strength of ≥1200MPa, an elongation after fracture of ≥15%, a cross-sectional shrinkage of ≥45%, a structure of pearlite + trace ferrite, a troostite rate of ≥85%, and no central martensite and grain boundary cementite.

[0052] The steel wire rope made of the hot-rolled wire rod for high-strength steel wire rope has a nominal tensile strength of ≥1870MPa, a torsion number of ≥25 times, and a bending number of ≥15 times.

[0053] After the application of the present invention, the product quality fully meets the requirements of relevant technical conditions and has been sent to the user for deep processing. After meeting the user's requirements, the annual production volume is expected to be about 10,000 tons. The benefit per ton of steel is calculated at 200 yuan, which can create economic benefits of 2 million yuan. It can be promoted and applied in the production of high-strength steel wire rope wire rods and other wire rods in various steel plants, and has good promotion and application prospects.

[0054] The solution of the present application is described below through specific embodiments.

[0055] Example 1 A wire factory adopts the technology of the present invention for production, and the specific implementation is as follows.

[0056] (1) A 200 mm × 200 mm ingot was obtained by converter smelting, LF refining and continuous casting. The superheat of the molten steel in the continuous casting process was 10-20 °C, the pulling speed was 1.4 m / min, the central carbon segregation of the ingot was 1.03-1.06, and the chemical composition was: C 0.60%, Si 0.40%, Mn 0.60%, P 0.015%, S 0.008%, Cr 0.30%; the rest was Fe and unavoidable impurities.

[0057] (2) The obtained ingot is heated in a heating furnace, the temperature of the heating furnace soaking section is 1000°C, and the heating time is 160 min.

[0058] (3) After heating, the ingot is dephosphorized by high-pressure water and then rolled on a high-speed wire with a starting rolling temperature of 920-940°C.

[0059] (4) During the rolling process, the opening degree of the 1# water tank is 25%, the outlet water pressure is 3.5 bar, and the flow rate is 25m 3 / h, the opening degree of 2# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 3# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 4# water tank is 20%, the outlet water pressure is 2.0 bar, and the flow rate is 18m 3 / h, the opening degree of 5# water tank is 5%, the outlet water pressure is 1.0 bar, and the flow rate is 5m 3 / h, the spinning temperature is 850℃.

[0060] (5) After spinning, the wire rod is cooled on the Stelmore air cooling line. The control parameters of the Stelmore air cooling line are as follows: the initial roller speed is 0.68 m / s, and the roller speed of the 2nd to 13th sections increases by 0.02 m / s; the opening degree of 1# to 4# fans is 100%, and the flow rate is 200,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 5# fan is 100%, and the flow rate is 160,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 6# fan is 80%, and the flow rate is 128,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 7# fan is 70%, and the flow rate is 112,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 8# fan is 60%, and the flow rate is 96,000 m 3 / h, the corresponding insulation cover is opened; the opening angle of the Jialing device is 5°; when it is quickly cooled to 600℃, it enters the insulation cover and turns off the fan, the cooling rate is 1.8℃ / s, and the coiling temperature is 400℃.

[0061] (6) The φ6.5mm wire rod produced by the above method has a tensile strength of 1200MPa, an elongation after fracture of 21%, a cross-sectional shrinkage of 50%, a structure of pearlite + trace ferrite, a troostite rate of 85%, and no central martensite and grain boundary cementite. The steel wire rope made of this wire rod has a nominal tensile strength of 1870MPa, a torsion number of 33 times, and a bending number of 17 times.

[0062] Example 2 A wire factory adopts the technology of the present invention for production, and the specific implementation is as follows.

[0063] (1) A 160 mm × 160 mm ingot was obtained by converter smelting, LF refining and continuous casting. The superheat of the molten steel in the continuous casting process was 15-25°C, the pulling speed was 1.8 m / min, the central carbon segregation of the ingot was 0.98-1.02, and the chemical composition was: C 0.70%, Si 0.80%, Mn 0.30%, P 0.011%, S 0.010%, Cr 0.10%; the rest was Fe and unavoidable impurities.

[0064] (2) The obtained ingot is heated in a heating furnace, the temperature of the heating furnace soaking section is 1050°C, and the heating time is 192 min.

[0065] (3) After heating, the ingot is dephosphorized by high-pressure water and then rolled on a high-speed wire with a starting rolling temperature of 950-980°C.

[0066] (4) During the rolling process, the opening degree of the 1# water tank is 25%, the outlet water pressure is 3.5 bar, and the flow rate is 25m 3 / h, the opening degree of 2# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 3# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 4# water tank is 20%, the outlet water pressure is 2.0 bar, and the flow rate is 18m 3 / h, 5# water tank opening degree is 5%, outlet water pressure ≤1.0bar, flow rate ≤5m 3 / h, and the spinning temperature is 885℃.

[0067] (5) After spinning, the wire rod is cooled on the Stelmore air cooling line. The control parameters of the Stelmore air cooling line are as follows: the initial roller speed is 0.68 m / s, and the roller speed of the 2nd to 13th sections increases by 0.02 m / s; the opening degree of 1# to 4# fans is 100%, and the flow rate is 200,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 5# fan is 100%, and the flow rate is 160,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 6# fan is 80%, and the flow rate is 128,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 7# fan is 70%, and the flow rate is 112,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 8# fan is 60%, and the flow rate is 96,000 m 3 / h, the corresponding insulation cover is opened; the opening angle of the Jialing device is 5°; when it is quickly cooled to 630℃, it enters the insulation cover and turns off the fan, the cooling rate is 2.5℃ / s, and the coiling temperature is 372℃.

[0068] (6) The φ6.5 mm wire rod produced by the above method has a tensile strength of 1280 MPa, an elongation after fracture of 15%, a cross-sectional shrinkage of 45%, a structure of pearlite + trace ferrite, a troostite ratio of 88%, and no central martensite and grain boundary cementite. The steel wire rope made of this wire rod has a nominal tensile strength of 1920 MPa, a torsion number of 25 times, and a bending number of 16 times.

[0069] Example 3 A wire factory adopts the technology of the present invention for production, and the specific implementation is as follows.

[0070] (1) A 150 mm × 150 mm ingot was obtained by converter smelting, LF refining and continuous casting. The superheat of the molten steel in the continuous casting process was 10-22°C, the pulling speed was 2.2 m / min, the central carbon segregation of the ingot was 0.98-1.04, and the chemical composition was: C 0.66%, Si 0.48%, Mn 0.53%, P ≤ 0.012%, S ≤ 0.007%, Cr 0.18%; the rest was Fe and unavoidable impurities.

[0071] (2) The obtained ingot is heated in a heating furnace, the temperature of the heating furnace soaking section is 1048°C, and the heating time is 180 min.

[0072] (3) After heating, the ingot is dephosphorized by high-pressure water and then rolled on a high-speed wire with a starting rolling temperature of 940-960°C.

[0073] (4) During the rolling process, the opening degree of the 1# water tank is 25%, the outlet water pressure is 3.5 bar, and the flow rate is 25m 3 / h, the opening degree of 2# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 3# water tank is 20%, the outlet water pressure is 3.0 bar, and the flow rate is 20m 3 / h, the opening degree of 4# water tank is 20%, the outlet water pressure is 2.0 bar, and the flow rate is 18m 3 / h, the opening degree of 5# water tank is 3%, the outlet water pressure is 0.8 bar, and the flow rate is 3m 3 / h, and the spinning temperature is 877℃.

[0074] (5) After spinning, the wire rod is cooled on the Stelmore air cooling line. The control parameters of the Stelmore air cooling line are as follows: the initial roller speed is 0.68 m / s, and the roller speed of the 2nd to 13th sections increases by 0.02 m / s; the opening degree of 1# to 4# fans is 100%, and the flow rate is 200,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 5# fan is 100%, and the flow rate is 160,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 6# fan is 80%, and the flow rate is 128,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 7# fan is 70%, and the flow rate is 112,000 m 3 / h, the corresponding insulation cover is open; the opening degree of 8# fan is 60%, and the flow rate is 96,000 m 3 / h, the corresponding insulation cover is opened; the opening angle of the Jialing device is 5°; when it is quickly cooled to 630℃, it enters the insulation cover and turns off the fan, the cooling rate is 2.2℃ / s, and the coiling temperature is 397℃.

[0075] (6) The φ6.5 mm wire rod produced by the above method has a tensile strength of 1265 MPa, an elongation after fracture of 19%, a cross-sectional shrinkage of 42%, a structure of pearlite + trace ferrite, a troostite ratio of 86%, and no central martensite and grain boundary cementite. The steel wire rope made of this wire rod has a nominal tensile strength of 1905 MPa, a torsion number of 30 times, and a bending number of 19 times.

[0076] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0077] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for preparing a hot-rolled wire rod for high-strength steel wire rope, characterized in that: include: The converter smelting, external refining and continuous casting are carried out in sequence to obtain the required ingots, and then the ingots are heated, dephosphorized with high-pressure water, rolled at a high speed, wire-laying machine, cooled by a Stelmore air-cooling line, coiled and packaged to obtain hot-rolled wire rods for high-strength steel wire ropes; wherein, during the rolling process, a plurality of water tanks are divided into a plurality of groups, and along the direction of the rolling production line, the opening degree, outlet pressure and flow rate of the plurality of water tanks are gradually reduced; during the controlled cooling process of the Stelmore air-cooling line, a plurality of fans are divided into a plurality of groups, and along the direction of the Stelmore air-cooling line, the opening degree of the plurality of fans is gradually reduced.

2. The method for preparing a hot-rolled wire rod for a high-strength steel wire rope according to claim 1, characterized in that: The chemical composition of the hot-rolled wire rod for high-strength steel wire rope is as follows by weight percentage: C: 0.60% to 0.70%, Si: 0.40% to 0.80%, Mn: 0.30% to 0.60%, P≤0.015%, S≤0.010%, Cr: 0.10% to 0.30%; the rest is Fe and unavoidable impurities.

3. The method for preparing the hot-rolled wire rod for high-strength steel wire rope according to claim 1, characterized in that: During the continuous casting process, the superheat degree of the molten steel is 10-25° C., the casting speed is constant, and the central carbon segregation degree of the ingot is 0.98-1.

06.

4. The method for preparing a hot-rolled wire rod for a high-strength steel wire rope according to claim 1, characterized in that: The heating of the ingot is carried out by a heating furnace, the temperature range of the soaking section of the heating furnace is 1000-1050°C, and the heating time t=(0.8-1.2)H, wherein H is the thickness of the ingot.

5. The method for preparing the hot-rolled wire rod for high-strength steel wire rope according to claim 4, characterized in that: The ingot is heated in the heating furnace and then dephosphorized by high-pressure water before being rolled into a wire rod on a high-speed wire. The rolling temperature is 920-980°C, and the rolling process is controlled by cooling water.

6. The method for preparing the hot-rolled wire rod for high-strength steel wire rope according to claim 5, characterized in that: During the rolling process, the opening degree of the 1# water tank is 20-30%, the outlet water pressure is 3-4 bar, and the flow rate is 20-30 m 3 / h, the opening degree of 2# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 3# water tank is 15~25%, the outlet water pressure is 2.5~3.5bar, and the flow rate is 15~25m 3 / h, the opening degree of 4# water tank is 15~25%, the outlet water pressure is 1.5~2.5bar, and the flow rate is 15~20m 3 / h, 5# water tank opening degree ≤10%, outlet water pressure ≤1.5bar, flow rate ≤10m 3 / h, the temperature before spinning is 850~885℃.

7. The method for preparing a hot-rolled wire rod for a high-strength steel wire rope according to claim 1, characterized in that: The wire rod after spinning is controlled cooled on the Stelmore air cooling line. The initial roller speed is 0.6~0.7m / s, and the speed of the 2nd to 13th rollers is increased by 0.01~0.03m / s.

8. The method for preparing the hot-rolled wire rod for high-strength steel wire rope according to claim 7, characterized in that: In the Stelmore air cooling line, the opening degree of 1#~5# fans is 95~100%, the opening degree of 6# fan is 75~85%, the opening degree of 7# fan is 65~75%, the opening degree of 8# fan is 55~65%, the insulation covers are all opened, and the opening angle of the Jialing device is 3~8°; when rapidly cooled to 600~630℃, the fans and insulation covers are turned off, and slow cooling is carried out at a cooling rate of ≤3℃ / s, and the coiling temperature is ≤450℃.

9. A hot-rolled wire rod for high-strength steel wire rope, characterized in that: The method is prepared by any one of claims 1 to 8.

10. The hot-rolled wire rod for high-strength steel wire rope according to claim 9, characterized in that: The hot-rolled wire rod for high-strength steel wire rope has a tensile strength of ≥1200MPa, an elongation after fracture of ≥15%, a cross-sectional shrinkage of ≥45%, a structure of pearlite + trace ferrite, a troostite rate of ≥85%, and no central martensite and grain boundary cementite.

Citation Information

Patent Citations

  • Method for controlling martensite and grain boundary cementite at center of 82B hot-rolled wire rod

    CN112080618A

  • Rolling method of high-carbon free-cutting steel wire rod

    CN113787094A

  • 82 / 86 / 92 grade tire cord steel wire rod and aging-free production method of tire cord steel wire rod

    CN114836592A

  • Novel controlled cooling process for reducing oxide scale of tire cord steel wire rod

    CN116984388A

  • Vanadium-containing hot-rolled wire rod for port machinery steel wire rope, production method of vanadium-containing hot-rolled wire rod and steel wire

    CN117089766A

Cited By

  • Production method and application of hot-rolled wire rod for high-strength and high-plasticity steel wire rope

    CN121198764A