Preparation method of bio-absorbable zinc-based silver-magnesium-calcium alloy

Through the preparation method of zinc-based silver magnesium calcium alloy, the problem of insufficient mechanical stability and high corrosion rate in the bone healing process is solved, and the mechanical properties and biocompatibility are improved. It is suitable for cardiovascular and orthopedic transplantation Entrance.

CN118996176APending Publication Date: 2024-11-22JIANGSU XIANGLAN MEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002789.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing zinc alloys have insufficient mechanical stability and high corrosion rate during bone healing, resulting in premature degradation of the implant and affecting bone reconstruction. The pure zinc is soft, brittle and has low mechanical strength.

Method used

The preparation method of zinc-based silver magnesium calcium alloy is adopted, including crucible melting, gravity casting, hot extrusion, cold rolling and annealing. By reasonably selecting alloy elements and processing methods, the mechanical properties and biocompatibility of the alloy are improved.

Benefits of technology

It significantly improves the mechanical properties and biocompatibility of zinc-based silver magnesium calcium alloy, is suitable for cardiovascular stents and orthopedic applications, extends the degradation time of the implant, and ensures mechanical stability and antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996176A_ABST
    Figure CN118996176A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a bio-absorbable zinc-based silver-magnesium-calcium alloy. The preparation method comprises the following steps: step 1, melting in a crucible; step 2, gravity casting; step 3, hot extrusion; 4, cold rolling; and 5, annealing. The preparation technology of the zinc-based silver-magnesium-calcium alloy provided by the invention is characterized in that a hot extrusion (HE) process is directly adopted after casting, and inter-process annealing is not needed; in addition, the influence of different thickness reduction, heat treatment (HT) time and temperature on structural evolution and mechanical properties of the Zn alloy in the cold rolling process is found, and the biodegradable high-strength multiphase Zn alloy is prepared; the invention has the beneficial effects that the preparation technology is simple, has the advantages of low cost, high efficiency and the like, and can be widely applied to the fields of medicine, aerospace, automobiles, electronic products and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of absorbable biomaterial preparation, in particular to a method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy. Background Art

[0002] Biodegradable metals are breaking the current research paradigm of biomaterials, and the requirements for mechanical properties, biocompatibility and corrosion resistance are getting higher and higher. Therefore, based on the previous research on magnesium-zinc alloys, we have recently conducted further research and development on zinc alloys and invented zinc-based silver-magnesium-calcium alloys. The following is an overview of the research and development background technology in this area;

[0003] Zinc is one of the trace elements in the human body and is involved in many important physiological and pathological processes. Pure zinc has recently been studied as a new type of biodegradable material; but pure zinc is soft, brittle and has low mechanical strength; zinc alloys have excellent biocompatibility and meet the required mechanical parameters; this is why they have attracted the attention of researchers; studies have found that zinc plays an important role in bone formation by activating aminoacyl-tRNA synthetases in osteoblasts, thereby increasing bone formation; zinc inhibits bone resorption by interfering with the formation of osteoclast-like cells; zinc also affects mesenchymal stem cells by increasing their growth rate and positively affecting their cell survival; in orthopedic studies, it was found that zinc supports the migration and cell proliferation of smooth muscle cells;

[0004] Silver has been intensively studied as an implant material and shows excellent biocompatibility. It has been shown that silver supports bone regeneration in cancellous bone and is therefore a promising choice for implant material. Silver improves the healing process after fractures by introducing silver nanoparticles; silver increases mesenchymal stem cell proliferation in mouse models. In addition, silver exhibits antibacterial properties by preventing bacteria from adhering to the material surface; this material property has been intensively studied in several medical fields to prevent bacterial infections after implantation.

[0005] Magnesium is one of the important trace elements in the human body. Magnesium-zinc-calcium alloys have good biophysical properties and biocompatibility. However, the high corrosion rate of magnesium (0.2-2 mm / year) and the formation of hydrogen cavitation in tissues are still problems in clinical applications. Excessive corrosion rate will lead to premature degradation of implant materials. Although this has been basically solved in the application of cardiovascular stents, it cannot guarantee sufficient mechanical stability during bone healing. In addition, the degradation of magnesium will lead to an increase in the pH value in the implant environment, thereby delaying bone reconstruction. Therefore, we further studied the performance of zinc-magnesium and other alloy materials based on zinc.

[0006] Our research found that the silver content of the zinc-silver alloy is related to the enhancement of mechanical properties, thereby changing the corrosion rate and biocompatibility; compared with the UTS of pure zinc of 115MPa, YS of 110MPa, and elongation at break of 9.7%, the UTS of the zinc-silver alloy is 211MPa, the yield strength (YS) is 213MPa, and the elongation at break is 25%; further research found that the ECAP sample of the Zn-3Ag-1Cu alloy has a high strength of 348MPa and a good ductility of up to 30%, showing its great potential as a promising material for the production of medical stents. Therefore, the present invention has deeply studied the mechanical properties of the zinc-based silver-magnesium-calcium alloy, and found that the mechanical properties, biocompatibility and corrosion resistance have been improved to a certain extent, which is suitable for the application requirements of clinical cardiovascular stents and orthopedics;

[0007] Silver (Ag) and magnesium as alloying additions to zinc not only help improve mechanical strength and ductility, but also have a positive impact on biological properties; we found that Mg 2+ When tested under in vitro conditions, the ion can positively affect the viability, proliferation, and adhesion of MG-63 cells; magnesium is an essential nutrient for the human body, with a recommended daily intake of between 320 and 400 mg; it promotes protein synthesis and acts as an activator of many enzymes; in addition, Mg 2+ Silver supports essential biological processes, including bone formation, by interacting with osteoblast integrins that load cell adhesion and stability. The most significant biological advantage of silver is that it enhances the antimicrobial activity of zinc alloys. Humans tolerate silver at levels of 0.4 to 27 μg / day.

[0008] Our previous studies have shown that the mechanical properties of Zn-3Ag-0.5Mg alloy meet the requirements of biodegradable implant materials. The best strength / ductility combination of cold-rolled Zn-3Ag-0.5Mg alloy reaches an ultimate tensile strength (UTS) of 430MPa, a yield strength (YS) of 380MPa, and a total elongation at break of 35% (εF); these mechanical properties are significantly higher than those required for implant applications: εF>15%, UTS>300MPa, YS>200MPa for stents, and YS>230MPa for fracture fixation; recent studies have shown that Zn-3Ag-0.5Mg alloy is also a promising material in terms of corrosion performance; uniform distribution The second phase precipitates form micro-cells in a fine-grained microstructure (high grain boundary density), resulting in uniform corrosion without substantial local corrosion; after a 6-month in vitro degradation study in Hanks solution, tiny pits formed over the entire sample surface resulted in a corrosion rate of 21.8 ± 0.4 μm / year; this value is higher compared to the degradation of pure zinc at 12.8 ± 0.2 μm / year; similar studies have been conducted on other biodegradable materials, and in general, accelerated corrosion of alloys compared to pure zinc was observed, however, when tested in the same salt-based environment, the values ​​for zinc alloys remained in the same order of magnitude, and the corrosion rates of zinc-based materials compared to other biodegradable metals were between those of magnesium and iron;

[0009] However, pure zinc is soft, brittle and has low mechanical strength. It is reported that the tensile strength of cast Zn is less than 20 MPa, the elongation is only 0.2%, and the Vickers hardness is 37. Therefore, further research is needed to achieve the desired mechanical properties. We developed a cast Zn-Mg alloy and studied its mechanical and corrosion behaviors. The results showed that 1% (wt.%) Mg alloying significantly improved the tensile strength of Zn, but the elongation of the cast ZnMg alloy was only 2%, although there was a significant improvement of 0.2% in the initial elongation of Zn.

[0010] The present invention selects nutrient elements (Mg, Ca and Ag) closely related to bone tissue as alloying elements of Zn; it is well known that Mg, Ca and Ag belong to the same group (IIA) in the periodic table and are important elements of bone matrix; magnesium regulates active calcium transport, thereby increasing bone mineral density and preventing fractures; calcium intake is one of the important modifiable environmental factors for normal bone development during growth and maintenance of bone mass in old age; the distribution of Ag is similar to that of Ca, 99% of the element is stored in the bones, which can inhibit bone resorption and stimulate bone formation in rodents and osteoporosis patients; therefore, based on the previous research and development, we invented a bioabsorbable zinc-based silver-magnesium-calcium alloy, which opened up a new path for application materials in the field of biodegradable metals. Summary of the invention

[0011] To achieve the above object, the technical solution of the present invention is a method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy, comprising the following steps:

[0012] Step 1: Crucible melting;

[0013] Step 2: Gravity casting;

[0014] Step 3: hot extrusion;

[0015] Step 4: cold rolling;

[0016] Step 5: Annealing.

[0017] As a further supplement to the technical solution, the crucible melting in step 1 is to melt commercial 99.99% pure zinc, silver (1-4% WT), magnesium (0.5-3% WT) and calcium (0.1-1% WT) in a graphite crucible at 650°C for 30-60 minutes to fully melt and fuse.

[0018] As a further supplement to the technical solution, the gravity casting in step 2 is to pour the molten alloy liquid in step 1 into a cold steel mold to prepare a steel ingot weighing about 250-2500 grams.

[0019] As a further supplement to the technical solution, the hot extrusion in step three is performed at 200-250° C. directly after gravity casting, and the extrusion ratio is equal to 25-15.

[0020] As a further supplement to the technical solution, the cold rolling in step 4 is to perform multiple steps of cold rolling on the material at a constant rolling speed of 0.006-0.06 m / s in a rolling mill, and the cold rolling thickness is reduced by 50%-90%.

[0021] As a further supplement to the technical solution, the annealing in step five is performed at 150-200° C. for 5-10 minutes after short-term deformation.

[0022] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy produces a stent which is used for implantation in cardiovascular and cerebrovascular vessels, peripheral blood vessels and hollow organs.

[0023] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy; the splints, screws or absorbable sutures prepared are used in orthopedic surgeries.

[0024] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy. The parts prepared are used in the fields of aerospace, automobile and electronic product technology.

[0025] The beneficial effect is that the zinc-based silver-magnesium-calcium alloy material provided by the present invention has excellent performance, simple preparation technology and process, low cost and high efficiency, and can be widely used in the fields of medicine, aerospace, automobiles and electronic products. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 .SE-SEM micrographs of Zn-3Mg HPT hybrids. AC: SE-SEM micrographs near the edge of the sample after 30 cycles of HPT+PDA (200℃, 1h). The blue dashed circles indicate the Mg-rich areas, which constitute the Mg2Zn11 phase; D, E, F: BSE-SEM micrographs of the HPT Zn-3Mg alloy near the edge of the sample after 1 cycle, 0.9 mm from the center after 5 cycles, and 1 mm from the center after 15 cycles; the Zn-rich (lighter contrast) and Mg2Zn11 (darker contrast) phases account for about 68% and 32% of the volume, respectively;

[0027] Figure 1-1 .SEM-BSE images of samples after HE (A), CR 30%, 50%, 75%, 90% (B–E), and CR90% followed by annealing for 15 min in longitudinal cross section (F);

[0028] Figure 2 Effect of magnesium content on the corrosion behavior of Zn-xMg, where x = 3, 10 or 30, HPT hybrid specimens were subjected to 15 cycles of: (a) open circuit potential (OCP), (b) potential dynamic polarization (PDP);

[0029] Figure 3 . Mechanical properties of pure Zn and Zn-1X (Mg, Ca, Ag) binary alloy and Zn-3Ag-1Mg-0.3Ca alloy: A: microhardness; B, C, D are tensile properties;

[0030] Figure 4 .Compression properties of extruded pure Zn and Zn-1X (Mg, Ca, Ag) binary alloy and Zn-3Ag-1Mg-0.3Ca alloy; A: stress-strain curve; B: compressive yield strength (YS);

[0031] Figure 5 .Microstructures of rolled pure Zn (A) and Zn-3Ag (B) and Zn-3Ag-1Mg-0.3Ca (C) alloys; green arrows indicate silver-rich precipitates, and yellow arrows indicate magnesium-rich precipitates;

[0032] Figure 6 . Cell adhesion experiment, SEM images of adhered single cells and corrosion products observed on the disk surfaces of pure Zn (A), Zn-3Ag (C), and Zn-3Ag-1Mg-0.3Ca (E) after incubation with MG-63 cells for 1 day; B, D, and F are magnified images of the blue arrowed areas, respectively;

[0033] Figure 7SEM and EDS (energy dispersive X-ray spectroscopy) results of cell adhesion and corrosion products; Surface morphology and EDS elemental maps (Zn, Ag, Mg, C, O, Ca, P, Cl) of Zn-based material discs and corrosion products formed on the surface directly after 1 day of incubation using MG-63 cells and SEM cell fixation procedures; Pure Zn (A); Zn-3Ag (B); Zn-3Ag-1Mg-0.3Ca (C); The points marked with asterisks are the points of EDS microchemical analysis;

[0034] Figure 8 . Endothelial cell culture adhesion morphology results. SEM photos of ECV304 cells cultured on pure magnesium, Zn-Ag-1Mg, Zn-3Ag-1Ca and Zn-3Ag-1Mg-0.3Ca alloys after 24 hours;

[0035] Fig. 9 . Morphological results of smooth muscle cell culture adhesion; SEM photos of VSMC cultured on pure magnesium, Zn-Ag-1Mg, Zn-3Ag-1Ca and Zn-3Ag-1Mg-0.3Ca alloys after 24 hours;

[0036] Fig.10 . showed the antibacterial properties of the zinc-based samples, and inhibition of bacterial growth was observed for all zinc-based samples; however, pure Zn( Fig.10 B) and Zn-3Ag alloy ( Fig.10 C) on the two bacteria than Zn-3Ag-1Mg-0.3Ca alloy ( Fig.10 D) is more significant, the control group is Ti( Fig.10 A). DETAILED DESCRIPTION

[0037] In order to make the technical solution more clear to those skilled in the art, Figure 1-10 The technical solution of the present invention is described in detail:

[0038] Based on the previous research and development, the present invention rationally optimizes the processing path based on the zinc-based binary alloy and ternary alloy, and invents a zinc-based silver-magnesium-calcium alloy material with mechanical properties that significantly exceed the requirements of biodegradable implant materials. The novelty of the present invention lies in the direct use of hot extrusion (HE) process after casting without the need for inter-process annealing. In addition, the effects of different thickness reductions, short-time heat treatment (HT) duration and temperature during cold rolling on the microstructure evolution and mechanical properties of Zn alloys were studied for the first time, and a biodegradable high-strength multiphase Zn alloy was prepared.

[0039] Sufficient plasticity is first provided by grain refinement, followed by a short annealing treatment to restore appropriate strength. We introduce alloying elements that provide solid solution strengthening and second phase strengthening to provide an appropriate platform for thermomechanical strengthening of Zn alloys, applying cold deformation processes to high-strength, brittle multiphase Zn alloys. In short, the full combination of CR reduction and subsequent HT provides meaningful plasticity improvement for high-strength, brittle HE Zn-based Ag-Mg-Ca alloys.

[0040] We provide mechanical properties that meet the requirements of biodegradable implant materials through the combined effects of grain refinement strengthening, second phase precipitation hardening, favorable texture, and an appropriate ratio of low-angle crystal phase (LAGB) and high-angle crystal phase (HAGB).

[0041] With the increase of CR ratio, the grain microstructure is the smallest ~0.76μm, with a typical rolling texture, and the deformation-induced precipitation ratio of ε-Zn3Ag phase is the highest. Through cold plastic deformation process and post-deformation annealing, the mechanical properties of the new zinc-based silver-magnesium-calcium alloy can be fine-tuned; the applied processing route can control the grain size, texture, second phase precipitation fraction and HAGB / LAGB density, thereby achieving a perfect combination of strength and plasticity in CR alloys;

[0042] Analysis of the annealing temperature dependence of HT application shows that the ultrafine-grained material obtained after CR90% exhibits high εF~200%, but insufficient mechanical strength (YS=162MPa, UTS=221MPa), which we improved by annealing after short-time deformation at 50°C; however, good mechanical strength (YS=372MPa, UTS=408MPa) and ductility (εF=34%) were found at 200°C. The best performance was obtained in the processing of CR50%+HT-5 samples, such as UTS of 430MPa, YS of 381MPa, and εF of 33%, which significantly exceeds the mechanical benchmarks of biodegradable implant materials (such as cardiovascular stents) and makes this material more valuable for biomedical applications, especially as an orthopedic application material.

[0043] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy comprises the following steps:

[0044] Step 1: Crucible melting;

[0045] Step 2: Gravity casting;

[0046] Step 3: hot extrusion;

[0047] Step 4: cold rolling;

[0048] Step 5: Annealing.

[0049] In the step 1, the crucible is melted, that is, commercial 99.99% pure zinc, silver (1-4% WT), magnesium (0.5-3% WT) and calcium (0.1-1% WT) are melted in a graphite crucible at 650° C. for 30-60 minutes to fully melt and fuse.

[0050] Among them, the gravity casting in step 2 is to pour the alloy liquid melted in step 1 into a cold steel mold to prepare a steel ingot weighing about 250-2500 grams.

[0051] Wherein, the hot extrusion in step 3 is performed directly at 200-250° C. after gravity casting, and the extrusion ratio is equal to 25-15.

[0052] Among them, the cold rolling in step 4 is to perform multiple steps of cold rolling on the material at a constant rolling speed of 0.006-0.06m / s in a rolling mill, and the cold rolling thickness is reduced by 50%-90%.

[0053] Wherein, the annealing in step 5 is annealing for 5-10 minutes after short-time deformation at 150-200°C.

[0054] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy produces a stent which is used for implantation in cardiovascular and cerebrovascular vessels, peripheral blood vessels and hollow organs.

[0055] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy; the splints, screws or absorbable sutures prepared are used in orthopedic surgeries.

[0056] A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy. The parts prepared are used in the fields of aerospace, automobile and electronic product technology.

[0057] like Figure 1 Shown are SE-SEM micrographs and mechanical property analysis of Zn-3Mg HPT hybrids.

[0058] SE-SEM micrographs of Zn-3Mg HPT hybrids. AC: SE-SEM micrographs near the edge of the sample after 30 cycles of HPT+PDA (200°C, 1h). The blue dashed circles indicate the Mg-rich areas, constituting the Mg2Zn11 phase. D, E, F: BSE-SEM micrographs of the HPTZn-3Mg alloy near the edge of the sample after 1 cycle, at 0.9 mm from the center after 5 cycles, and at 1 mm from the center after 15 cycles; the Zn-rich (lighter contrast) and Mg2Zn11 (darker contrast) phases account for approximately 68% and 32% of the volume, respectively.

[0059] After PDA, the microstructure shows no macroscopic evidence of different phases. It should be noted that after PDA, the large Mg-rich phase present in the central region of the sample after 30 cycles is no longer distinguishable; however, high-magnification SE-SEM micrographs show that the grain size of the Zn-rich and Mg-rich phases is approximately 700nm or larger. Notably, this is approximately 3 times the grain size before PDA treatment. Figure C shows that the Mg-rich area, highlighted by the blue dashed circle, is haphazardly scattered with lightweight nanoscale precipitates. High-magnification BSE-SEM micrographs of the microstructure of the Zn-3Mg alloy are shown in Figure . Figure 1 DF. The volume percentage of the zinc-rich phase is about 68%. The rest of the microstructure (~32 volume percent) contains the Mg2Zn11 phase region.

[0060] Figure 1 The microhardness of pure Zn and Zn-1X (Mg, Ca, Ag) binary alloys in cast (A) and rolled (B) conditions is shown. It can be seen that the hardness of pure Zn in cast state is quite low, only (38.24±1.06)Hv, but after alloying with Mg, Ca, and Ag elements, the microhardness is significantly increased to (78.26±2.84)Hv (pure Zn in cast state). Zn-1Mg), (73.00±7.43)Hv (Zn-1Ca in cast state), and (61.88±6.72)Hv (Zn-1Sr in cast state). The microhardness of rolled Zn-1X alloy shows a similar trend to that of cast alloy.

[0061] like Figure 1-1 Shown, ultrastructural analysis; SEM-BSE images of samples after HE (A), CR 30%, 50%, 75%, 90% (B–E), and CR90% followed by annealing for 15 min in longitudinal cross-section (F).

[0062] After HE processing, the microstructure of Zn-3Mg alloy consists of a Zn-rich matrix with Mg2Zn11 grain sizes ranging from ∼100 to 300 nm. HRTEM images confirm the presence of nanocrystalline domains. On PDA, the average grain size of the alloy increases to ∼700 nm. Mg2Zn11 nanoscale intermetallic compounds, either aggregated between adjacent Zn grains or distributed along grain boundaries after HPT, diffuse and coalesce into larger grains during PDA. The volume percentages of Zn and Mg2Zn11 are estimated to be 68% and 32%, respectively, which are close to the theoretical equilibrium composition of 57Zn-43Mg2Zn11 in Zn-3Mg.

[0063] like Figure 2As shown, the electrochemical test was carried out in Hank's solution at 37°C on an electrochemical workstation (CHI 604D). Before the electrochemical test, the sample surface was polished; a three-electrode cell was used for electrochemical measurement; the auxiliary electrode was platinum and the reference electrode was a saturated calomel electrode (SCE); the open circuit potential (OCP) was monitored for 7200 seconds; the potentiodynamic polarization test was carried out at a scan rate of 1 mV / s, and the initial potential after OCP measurement was about 300 mV lower than the corrosion potential (Ecorr); the measurement area was 0.385 cm 2 (Φ7 mm); Three measurements were performed for each sample group; The Tafel area of ​​the polarization curve was analyzed to obtain the corrosion current density (icorr) of pure Zn and Zn-1X alloy (by linear fitting and Tafel extrapolation to the cathodic and anodic parts of the polarization curve); The in vitro corrosion rate calculated by electrochemical measurement converted icorr into corrosion rate according to Faraday's law: C = Micorr / nFρ, where C is the corrosion rate in mm / year, M is the molar mass, n is the number of electrons involved in the corrosion reaction, F is the Faraday constant, and ρ is the density of the material; Finally, we found that higher Mg content was associated with a decrease in corrosion potential and an increase in current density, indicating that the galvanic coupling is highly sensitive to corrosion; As the Mg content in the alloy increases, the proportion of Mg available for corrosion also increases; The increase in effective Mg atoms amplifies the potential for electrochemical reactions, resulting in more pronounced electrochemical reactions. This explains the observed trend of decreased corrosion potential and increased corrosion current density with increasing Mg content.

[0064] like Figure 3 As shown, the microhardness and tensile properties of the material are analyzed. Figure 3Figure A shows the microhardness of pure Zn, Zn-1X (Mg, Ca, Ag) binary alloy and Zn-3Ag-1Mg-0.3Ca alloy in cast state; Figure B, C, D show the tensile properties of pure Zn and Zn-1X (Mg, Ca, Ag) binary alloy and Zn-3Ag-1Mg-0.3Ca alloy in cast state, rolled state and extruded state respectively. Obviously, the yield strength (YS), ultimate tensile strength (UTS) and elongation of pure Zn in cast state are relatively low, which are only (10.14±2.32)MPa, (18.25±2.99)MPa and (0.32±0.08)% respectively. After adding alloying elements Mg, Ca and Ag, the YS, UTS and elongation of the as-cast Zn-1X binary alloys were significantly improved to (127.98±10.72)MPa, (184.84±20.91)MPa and (1.82±0.23)% (Zn-1Mg); (119.12±7.01)MPa, (164.57±13.92)MPa and (2.10±0.23)% (Zn-1Ca); (120.21±6.08)MPa, (171.40±14.13)MPa and (2.03±0.22)% (Zn-3Ag); after cold rolling, the YS, UTS and elongation of the Zn-1X binary alloys were further improved. Similar to the cold rolling process, the hot extrusion process also improved the tensile properties of the Zn-1X alloys.

[0065] like Figure 4 As shown, in order to improve the mechanical properties of pure zinc, the present invention tests two commonly used methods in metal material processing: adding alloy elements and processing deformation. Figure 4 As shown, both methods perform well; Figure 4 A shows the compression properties of pure Zn and Zn-1X (Mg, Ca, Ag) binary alloys and Zn-3Ag-1Mg-0.3Ca alloys. From the compressive stress-strain curves, the Zn-1X binary alloys show unique superplastic characteristics under compression, which can be explained by the formation of compression twins. Due to the compressive superplastic characteristics of the Zn-1X binary alloy, we cannot obtain the ultimate compressive strength, but only the yield strength under compression. Figure 4B shows the compressive yield strength data of pure Zn and Zn-1X binary alloy and Zn-3Ag-1Mg-0.3Ca alloy. It is obvious that the compressive yield strength increases from (102.92±6.73)MPa of pure Zn to (284.50±16.90)MPa(Zn-1Mg), (280.70±20.72)MPa(Zn-1Ca), (280.68±17.70)MPa(Zn-3Ag), (336.98±17.70)MPa(Zn-3Ag-1Mg-0.3Ca), indicating that alloying (Mg, Ca and Ag elements) effectively improves its mechanical properties.

[0066] Mechanical properties are a very important factor for biodegradable metals. Implants such as bone plates and vascular stents are used to replace human tissues, and their mechanical properties should match those of local tissues or organs or the environment.

[0067] like Figure 5 As shown, the microstructure analysis of zinc-based materials, Figure 5 A shows the SEM image of the pure Zn microstructure; Figure 5 B, C show the SEM images of the microstructure of Zn-3Ag and Zn-3Ag-1Mg-0.3Ca alloys, respectively. The microstructure of Zn consists of recrystallized equiaxed grains with relatively large grain size after the plastic deformation process. The white precipitate marked with a green arrow in Figure C belongs to the ε-Zn3Ag phase. In the Zn-3Ag-1Mg-0.3Ca alloy, the precipitate visible as the black area and marked with a yellow arrow is rich in Mg and is either Zn2Mg or Zn1.94Ag0.06Mg phase according to the proposed XRD, which is consistent with our previous study. It is obvious that the alloying addition refines the grain size and helps in the formation of a multiphase microstructure. This fine microstructure is beneficial for a uniform biodegradation process in physiological solutions, as excessive localized corrosion may lead to a catastrophic loss of the mechanical integrity of the implant in contact with the damaged tissue.

[0068] like Figure 6The SEM images shown in the figure show the SEM images of adhered single cells and corrosion products observed on the disk surfaces of pure Zn (A), Zn-3Ag (C), and Zn-3Ag-1Mg-0.3Ca (E) after incubation with MG-63 cells for 1 day. B, D, and F are magnified images of the blue arrows, respectively. Immersing the cell-seeded alloys in CCM and / or using cell seeding to adhere to the alloy surface will lead to the formation of corrosion products with small, spherical shapes that barely adhere to the surface, indicating cell death. Only single cells were present on the pure Zn and Zn-3Ag alloys, and the number of cells on the surface of the Zn-3Ag-1Mg-0.3Ca alloy was slightly higher; the results of the changes in cell viability over time when MG63 cells were cultured with various experimental material extracts. It can be seen that the pure Zn extract leads to a significant decrease in cell viability (*p < 0.05), however, the addition of alloying elements Mg, Ca, and Ag to Zn can significantly increase the number and viability of MG63. Compared with the pure Zn group and the negative control group, it can promote the proliferation of MG63 cells. Moreover, the alloy element Ag has the best effect in promoting the proliferation of MG63 cells, followed by Ca and then Mg.

[0069] like Figure 7 As shown in Figure 2, SEM-EDS analysis reveals the chemical composition of corrosion products formed on the surface of zinc-based samples after incubation with cells. Figure 7 From the element distribution shown in , it can be seen that the corrosion products are only a few microns in size. They are spherical, with some of them having a more developed needle-like morphology. The EDS point analysis results show that the corrosion products are mainly composed of Zn, O, C, and contain trace amounts of P. The EDS spectrum collected from the "bare" metal area shows a thin surface layer composed of O and C and small amounts of Cl and Ca (excluding the elements that make up the sample). The obvious difference in Ag and Mg concentrations in the Zn-3Ag and Zn-3Ag-1Mg-0.3Ca alloys is caused by the presence of silver-rich particles within the electron beam interaction volume during the EDS analysis.

[0070] like Figure 8, 9 shows the viability of ECV304 cells and VSMC cells cultured in pure Zn and Zn-1X alloy and Zn-3Ag-1Mg-0.3Ca alloy extract medium for 1, 3 and 5 days. For ECV304 cells, Zn-3Ag-1Mg-0.3Ca alloy showed significantly higher cell viability compared with Zn-1X alloy group and pure Zn group; while for VSMC cells, alloy elements had no obvious promoting effect. It can be seen that pure Zn extract leads to a significant decrease in cell viability compared with the negative control (*p < 0.05), however, adding alloy elements Mg, Ca and Ag to Zn can significantly improve cell viability. Compared with the pure Zn group and the negative control group, it can promote cell proliferation. Moreover, the alloy element Ag has the best effect in promoting cell proliferation, followed by Ca, and then the alloy element Mg.

[0071] It is obvious that cells cultured on pure Zn showed an unhealthy morphology, most of the cells were round and dead, and only a few cells were healthy polygonal or spindle-shaped. However, ECV304 and VSMC cells on the Zn-1X alloy surface had healthy morphology, most of them were polygonal or spindle-shaped, spread and proliferated well, and also showed abundant pseudopodia and secreted extracellular matrix. Unlike ECV304 cells, VSMC cells did not adhere, spread and proliferate on the surface of all experimental groups. VSMC cells showed unhealthy round and dead morphology on the pure Zn and Zn-1X alloy surfaces. This indicates that the addition of Mg, Ca and Ag alloying elements to Zn does not improve cell adhesion and the viability and proliferation of VSMC. This inhibitory effect on VSMC has the effect of preventing restenosis after implantation of intravascular stents.

[0072] like Fig.10 As shown, Fig.10 The antibacterial properties of the zinc-based samples were shown. Inhibition of bacterial growth was observed for all zinc-based samples. However, pure Zn( Fig.10 B) and Zn-3Ag alloy ( Fig.10 C) on the two bacteria than Zn-3Ag-1Mg-0.3Ca alloy ( Fig.10 D) is more significant, the control group is Ti( Fig.10 A); Ag addition resulted in a significant inhibition of bacterial growth in the Zn-3Ag alloy, with an inhibition rate of more than 90%; the inhibition rate in the pure zinc group was 57%; the inhibition rate in the Zn-3Ag-1Mg-0.3Ca alloy group was 35%. In addition, the antibacterial activity depended on the bacterial strain analyzed, with the antibacterial effect against Staphylococcus aureus being ~30% more pronounced than against Escherichia coli. No antibacterial effect was observed around the Ti sample used as a reference.

[0073] In summary, we found that by adding alloying elements such as Mg, Ca, and Ag, Zn-1X alloys greatly improved the mechanical properties, corrosion behavior, and biocompatibility of pure Zn. Zn-1X binary alloys and zinc-based silver-magnesium-calcium alloys showed great application potential in the field of new generation metal materials. They can be used as cardiovascular stents and biodegradable implants in orthopedics, opening up a new path for the application of materials in the field of biodegradable metals.

[0074] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy, characterized in that: The following steps are involved: Step 1: Crucible melting; Step 2: Gravity casting; Step 3: hot extrusion; Step 4: cold rolling; Step 5: Annealing.

2. The method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to claim 1, characterized in that: In the step 1, the crucible is melted, that is, commercial 99.99% pure zinc, silver (1-4% WT), magnesium (0.5-3% WT) and calcium (0.1-1% WT) are melted in a graphite crucible at 650° C. for 30-60 minutes to fully melt and fuse.

3. The method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to claim 2, characterized in that: The gravity casting in step 2 is to pour the alloy liquid melted in step 1 into a cold steel mold to prepare a steel ingot weighing about 250-2500 grams.

4. The method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to claim 1, characterized in that: The hot extrusion in step three is performed directly at 200-250° C. after gravity casting, and the extrusion ratio is equal to 25-15.

5. The method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to claim 1, characterized in that: The cold rolling in step 4 is to perform multiple steps of cold rolling on the material at a constant rolling speed of 0.006-0.06 m / s in a rolling mill, and the cold rolling thickness is reduced by 50%-90%.

6. The method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to claim 1, characterized in that: The annealing in step 5 is performed at 150-200° C. for a short time and then annealed for 5-10 minutes.

7. The stent prepared by the method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to any one of claims 1 to 6 is used for implantation in cardiovascular and cerebrovascular vessels, peripheral blood vessels and hollow organs.

8. The splint, screw or absorbable suture obtained by the preparation method of a bioabsorbable zinc-based silver-magnesium-calcium alloy according to any one of claims 1 to 6 is used in orthopedic related surgeries.

9. The parts obtained by the method for preparing a bioabsorbable zinc-based silver-magnesium-calcium alloy according to any one of claims 1 to 6 are used in the fields of aerospace, automobile and electronic product technology.