High-end free-cutting stainless steel for precision mechanical parts and preparation method of high-end free-cutting stainless steel
By optimizing the chemical composition and smelting process of stainless steel, appropriate ferrite and composite sulfide are formed, and the problem of existing easy-to-cut stainless steels taking into account the corrosion resistance and turning properties is achieved, and high corrosion resistance and excellent turning are achieved. High performance and material yield, suitable for the application of precision mechanical parts.
Patent Information
- Application Number
- CN202411023010.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to take into account the corrosion resistance and turning properties of existing easy-to-cut stainless steels, especially in the application of precision mechanical parts, pit problems often occur after surface polishing, which affects aesthetics and corrosion resistance.
By optimizing the chemical composition of stainless steel, including controlling the proportion of carbon, silicon, manganese, sulfur, nickel, chromium, copper, molybdenum, nitrogen, magnesium and rare earth elements, the appropriate ferrite and composite sulfides are formed, combining aluminum and silicon Combined with deoxygenation, modified oxidation inclusions, a multi-step smelting and rolling process is adopted to ensure uniform distribution of sulfides and low oxygen content.
It achieves high corrosion resistance, excellent turning performance, smooth and pit-free polishing surface, excellent hot-processed surface quality, and has a material yield of more than 90%. It is suitable for the production of complex parts with high requirements for corrosion resistance and surface aesthetics.
Smart Images

Figure CN118996281A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel manufacturing, and relates to a free-cutting stainless steel and a manufacturing method thereof, and in particular to a high-end free-cutting stainless steel for precision mechanical parts and a manufacturing method thereof. Background Art
[0002] Free-cutting stainless steel is widely favored by the market due to its good corrosion resistance and turning processability. Free-cutting stainless steel refers to stainless steel with good cutting performance by adding appropriate chemical elements that can improve cutting performance. Commonly used free-cutting stainless steel mainly obtains good cutting performance by adding free-cutting element sulfur. Sulfur combines with manganese in steel to form brittle and low-hardness manganese sulfide. Manganese sulfide can act as a stress concentration source during the cutting process, reducing cutting force and thus improving turning performance. In order to obtain evenly distributed manganese sulfide, people often control the oxygen content in the steel to form high-content oxide inclusions in the steel, such as Al2O3, SiO2, CaO, etc. These inclusions will become nucleation points for sulfides, allowing the sulfides to be evenly distributed in the stainless steel. The most harmful of these inclusions is the Al2O3 inclusion. Al2O3 itself has a high melting point and high hardness, which reduces the life of the tool and the turning performance during material cutting. When polishing the stainless steel surface, Al2O3 will fall off to form tiny "pits", affecting the surface aesthetics and corrosion resistance of precision parts.
[0003] In order to solve such problems, relevant documents were searched and a Chinese patent with publication number CN 110656280A disclosed "Low-oxygen calcium-magnesium-containing sulfur-based free-cutting steel and its preparation method". The invention reduces the oxygen content and adds Ca and Mg elements, ultimately forming dispersed composite sulfides with appropriate particle size and containing a hard core in the steel, thereby improving the anisotropy of the steel while ensuring the turning performance of the steel. The composite treatment of Ca and Mg will have a better effect than adding either of them alone, but if the increase of Ca and Mg is not enough, the modification of oxides such as Al2O3 will not be thorough, and if too much is added, it is easy to form high-melting point compounds, thereby blocking the water nozzle, which is not conducive to continuous casting production.
[0004] The Chinese patent with publication number CN 110117694A discloses a "magnesium addition process for magnesium-containing free-cutting steel". The invention provides a method for adding magnesium to sulfur-containing steel. By adding the Mg element, the sulfide is dispersed and evenly distributed, thereby improving the machinability. However, there is also a situation where the modification of oxide inclusions is not complete.
[0005] The Chinese patent with publication number CN 1456699 A discloses "a calcium rare earth tin composite free-cutting steel". The invention provides a new type of Ca-Re-Sn composite free-cutting steel. The performance and turning tests show that the surface material has excellent mechanical properties and improved turning performance, but excessive addition of tin will have a certain impact on hot processing.
[0006] The Chinese patent with publication number CN 112095051 A discloses "free-cutting steel treated with magnesium calcium tellurium composite treatment and its preparation method and application". This invention achieves uniform distribution of sulfides, reduces the aspect ratio of sulfides, and improves turning performance by composite addition of magnesium calcium tellurium. It can achieve good results in conventional stainless steel. Coarse sulfides will also reduce the corrosion resistance of the material and are not suitable for addition to stainless steel. It can be seen that there is still room for improvement in the current field for free-cutting stainless steel, especially for high-end free-cutting stainless steel used for precision machinery parts. Summary of the invention
[0007] In order to solve the problems of the prior art, the purpose of the present invention is to provide a high-end free-cutting stainless steel for precision machinery parts and a method for making the same, wherein the stainless steel has the following advantages: 1) high corrosion resistance, no rust in a neutral salt spray test for 240 hours; 2) excellent turning performance, solving the problem that corrosion resistance and free-cutting properties cannot coexist in stainless steel; 3) excellent polishing surface quality: the surface of the material is smooth and free of pits after subsequent turning and polishing; 4) excellent surface quality of the material during hot processing, and the preparation method provided by the present invention has a high yield rate.
[0008] To achieve the above objectives, the technology of the present invention adopts the following technical measures.
[0009] The invention provides a high-end free-cutting stainless steel for precision machinery parts, characterized in that, in terms of mass percentage, the chemical composition of the stainless steel comprises: carbon (C) ≤ 0.03%; silicon (Si) 0.2%-1.0%; manganese (Mn) 1.0%-2.0%; phosphorus (P) ≤ 0.05%; sulfur (S) 0.08%-0.18%; nickel (Ni) 12.0%-14.0%; chromium (Cr) 16.0%-18.0%; copper (Cu) 0.20%-0.60%; molybdenum (Mo) 2.0%-3.0%; nitrogen (N) 0.02%-0.1%; magnesium (Mg) 0.0004%-0.006%; rare earth (Re) 0.001%-0.010%, and the rest is iron and unavoidable impurities.
[0010] Preferably, by mass percentage, the carbon (C) content is below 0.028%; the silicon (Si) content is between 0.3% and 0.8%; the manganese (Mn) content is between 1.2% and 1.8%; the phosphorus (P) content is below 0.045%; the sulfur (S) content is between 0.09% and 0.12%; the nickel (Ni) content is between 12.3% and 13.0%; the chromium (Cr) content is between 16.5% and 17.5%; the copper (Cu) content is between 0.30% and 0.50%; the molybdenum (Mo) content is between 2.3% and 2.8%; the nitrogen (N) content is between 0.02% and 0.08%; the magnesium (Mg) content is between 0.0006% and 0.005%; the rare earth (Re) content is between 0.002% and 0.008%, and the rest is iron and unavoidable impurities.
[0011] A high-end free-cutting stainless steel for precision mechanical parts, wherein the chemical composition of the stainless steel is adjusted to meet the ferrite (DFW): 1 to 7, more preferably the ferrite (DFW): 1.5 to 7, more preferably the ferrite (DFW): 2 to 6.5; wherein,
[0012] DFW=138-99.7×(30×C%+30×N%+0.5×Mn%+Ni%+36.5) / (1.5×Si%+Cr%+Mo%+17.6)
[0013] Each element in the formula represents its percentage content in stainless steel.
[0014] The element design ideas of the present invention are:
[0015] The C content is controlled below 0.03%. C in steel mainly plays the role of stabilizing austenite and improving the strength of stainless steel. However, carbon easily forms various carbides, which reduce the corrosion resistance and plasticity of the material. Therefore, in order to retain the plasticity of the material and improve the corrosion resistance, C is required to be as low as possible. Austenite stability may be achieved through other elements such as Mn and Ni.
[0016] The Si content is controlled between 0.2-1.0%. Si is a residual element in silicon-deoxidized steel. In order to reduce the oxygen content in the molten steel, a certain content of Si is required. However, too high Si will cause the material to become brittle. Moreover, Si is a strong ferrite-forming element, which is not conducive to the stability of austenite.
[0017] The Mn content is between 1.0-2.0%. On the one hand, Mn is a stabilizing element of austenite, and on the other hand, it can also improve the strength of stainless steel. At the same time, Mn is an indispensable element in sulfur-containing steel. It can form MnS inclusions with S. When turning, MnS can serve as a fracture source to reduce the turning force and lubricate the tool, thereby improving the turning performance of the material. However, Mn should not be too high. Too high Mn will inevitably cause excessive strength and difficulty in processing, and Mn can promote the precipitation of σ phase, causing the steel to be brittle.
[0018] The P content is below 0.050%. P is a harmful element in stainless steel and is generally required to be as low as possible.
[0019] The S content is between 0.08% and 0.18%. S is the main element of free-cutting steel. The sulfide formed by S in the steel is the key to free-cutting. Generally speaking, the higher the sulfur content, the easier it is to turn. However, the addition of sulfur will bring many problems because the sulfide itself is an inclusion and it has all the adverse effects of inclusions. The optimization scope of the present invention is to maximize the free-cutting effect of S while preventing it from having too great an impact.
[0020] The Cr content is between 17.0-18.0%. Cr is the main element in stainless steel that plays a role in stainless steel. The higher the Cr content, the better the stainless effect. However, Cr is a ferrite-forming element. Too high Cr is not conducive to the stability of austenite and will also bring about the problem of excessive strength.
[0021] The Ni content is between 12.0-14.0%. Ni is an important element for the formation of austenite. It can significantly improve the corrosion resistance of stainless steel when combined with Cr, and Ni can improve the plasticity of stainless steel. However, Ni is relatively expensive. The amount of Ni to be added in austenite is generally determined based on the Cr content.
[0022] The Cu content is between 0.20% and 0.60%. Cu is a weaker austenite-forming element and plays a certain role in strengthening austenite. Its greatest role is to improve the cold heading performance of the material, increase its deformability and plasticity. At the same time, Cu can also appropriately improve the corrosion resistance of stainless steel, but too high Cu will also reduce the hot processing performance of the material.
[0023] The Mo content is between 2.0% and 3.0%, which is an element that promotes the formation of ferrite. Adding Mo is an important means to further improve the corrosion resistance of stainless steel, especially in some sulfur-containing steels. It can reduce the adverse effects of S on corrosion resistance. At the same time, Mo will increase the strength of the material after being dissolved in the matrix. However, if the content is too high, it will easily form various second phase products with the matrix elements, seriously affecting the performance.
[0024] The N content is between 0.02% and 0.1%. N is a strong austenite stabilizing element and is mainly used to adjust the ferrite content in steel. At the same time, it increases the strength of the material and can reduce the precipitation of σ phase to prevent high temperature brittleness. However, too high a content will reduce the thermoplasticity, so it is necessary to optimize the control.
[0025] The Mg content is between 0.0004% and 0.006%, which is generally not contained in conventional stainless steel. Its solubility in stainless steel is low, and it generally exists in the steel in the form of inclusions. In sulfur-containing stainless steel, Mg is easily combined with oxygen to form MgO inclusions, and is also easily combined with Al2O3 to form Mg-Al-O composite inclusions, which can serve as a source of manganese sulfide, making the sulfide evenly distributed in any corner of the steel. At the same time, Mg should not be too high. Too high Mg will form high-melting-point compounds, affecting the turning performance and blocking the water outlet.
[0026] The Re content is between 0.001% and 0.010%. Rare earths are widely used in steel, and the most common function is to purify molten steel. In the present invention, Re has two main functions: one is to eliminate or reduce the problem of poor hot working performance and plasticity caused by adding Mg; the other is that Re has a strong affinity for oxygen and sulfur, and can effectively modify sulfides and oxides to further improve turning performance.
[0027] The ferrite (DFW) content of the present invention is controlled mainly to improve the yield of the material. A certain ferrite content will help dissolve the unfavorable intermetallic compounds of the steel grade, thereby improving thermoplasticity and reducing rolling cracking. However, the ferrite content cannot be too much, as excessive ferrite is harmful to thermoplasticity.
[0028] Each element has a specific role in stainless steel, but the design of a single element cannot fully achieve the expected effect, and the coordination of multiple elements is required. In the design of the present invention, in order to improve the turning performance of the material, S, Mg, and Re free-cutting elements are added, and a certain content of Mn is combined to form composite inclusions such as Mg-Al-O-MnS, Mg-Si-O-MnS, and Re-MnS, so as to achieve the best sulfide morphology and distribution, reduce cutting force, and the modification of inclusions also reduces the influence of S on corrosion resistance. At the same time, corrosion-resistant elements such as Cr, Ni, and Mo are added to make the material have higher corrosion resistance.
[0029] Another important problem solved in the present invention is the smoothness of sulfur-containing steel after polishing. Conventional sulfur-containing steel allows some oxygen to exist in the steel to improve the dispersion of sulfides, which inevitably leads to the presence of more oxide inclusions. During the polishing process, these oxides will form surface pits, which seriously affect the appearance and corrosion resistance of the product. The present invention adopts aluminum and silicon combined deoxidation to control the oxygen content after refining to ≤30ppm, and adds Mg and Re to modify the oxide inclusions in the residual molten steel into softer silicate inclusions and rare earth inclusions. The modified inclusions have less effect on the polishing surface quality and corrosion resistance.
[0030] In order to prevent rolling cracking and improve the material rolling yield, the present invention controls the ferrite (DFW): 1 to 7, improves the hot processing performance of the material, and fully heats the billet before rolling to make the temperature of the billet uniform before rolling and reach the optimal thermoplastic temperature. The rolling temperature is controlled to prevent the head from splitting and causing the yield rate to decrease. The rolling process adopts head water-avoiding rolling, and the process uses induction heating to supplement the temperature to prevent the temperature from dropping too much, which is not suitable for thermal deformation and causes cracking, so that the material is rolled without cracking or splitting, and the yield rate is high. The present invention achieves an effective improvement in the yield rate through the comprehensive regulation of each step of the preparation method, wherein the yield rate can reach more than 90% when the DFW is controlled at 1 to 7, and the yield rate can be further increased to more than 94% when it is regulated to 1.5 to 7, and can even be regulated to 2 to 6.5 to increase the yield rate to more than 95%, so as to meet higher production process requirements.
[0031] The present invention also provides a method for preparing high-end free-cutting stainless steel for precision machinery parts, the method comprising: smelting, casting, rolling and heat treating the raw materials to obtain the high-end free-cutting stainless steel. More preferably: the smelting process comprises electric furnace smelting, AOD smelting and LF refining; casting by continuous casting; rolling by high-speed wire rolling unit; and solid solution by an annular solid solution furnace.
[0032] More preferably, the AOD smelting process controls the oxygen content to ≤30 ppm.
[0033] More preferably, after adjusting the elements other than Mg and Re in the molten steel to meet the composition requirements during LF refining, the iron cored wire containing magnesium powder and rare earth is fed to adjust the Mg and Re contents of the molten steel to reach the target values; more preferably, the iron cored wire comprises pure magnesium wire and rare earth wire, or an iron cored wire containing both magnesium powder and rare earth; more preferably, the molten steel temperature is readjusted to 1600-1630°C before wire feeding, which is beneficial to improving the recovery rate of Mg and Re.
[0034] More preferably, each step specifically includes the following:
[0035] Electric furnace smelting: Use scrap stainless steel with P≤0.035% to melt into crude molten steel. After smelting, add 6-10 kg of ferrosilicon per ton of molten steel for reduction. After the reduction is completed, remove all the slag, add 5-8 kg of carbonized rice husk per ton of molten steel for heat preservation and then tap the steel. The tapping temperature is 1600-1640℃;
[0036] AOD smelting: First, oxygen decarburization process is carried out, using high-temperature carbon blowing, the temperature is controlled at 1690-1750℃, the time is controlled at 35-45min, the slag basicity is controlled at 2.5-3.5, and the decarburization end point C is guaranteed to be ≤0.01%; secondly, the reduction process is carried out, 20-40Kg of ferrosilicon is added per ton of molten steel, the temperature is controlled at 1600-1680℃, the time is 8-15min, and the slag basicity is controlled at 1.0-2.5; then refining is carried out again During the refining process, 1-1.5 kg / ton of pure aluminum ingots are added for deep deoxidation. The oxygen content in the steel is ≤25 ppm after refining. The refining time is 8-12 minutes, the temperature is 1600-1650°C, and the slag basicity is 1.0-2.5. In the later stage of refining, sufficient ferrosulphur is added at one time according to the amount of molten steel, so that the S content of the molten steel meets the target value S: 0.08-0.18%. Finally, the temperature is adjusted to 1580-1620°C, and the molten steel is removed for the next step.
[0037] LF refining: After the molten steel arrives at the station, the temperature is measured and sampled, and the temperature is adjusted to 1620-1650℃. According to the current stainless steel structure, by adding pure iron, ferrochrome, ferronickel, ferrosilicon, pure manganese, ferrosulphur, pure copper, and ferromolybdenum, the elements other than Mg and Re are adjusted to meet the composition requirements, and then the molten steel temperature is readjusted to 1600-1630℃, and pure magnesium wire and rare earth wire are fed. The pure magnesium wire and rare earth wire are iron sheet cored wires with a diameter of 9-12mm, with magnesium powder and rare earth inside and iron sheet outside; magnesium powder and rare earth can also be mixed in the same iron sheet cored wire for wire feeding; the Mg and Re contents of the molten steel are adjusted to reach the target values, and then the temperature is adjusted to 1560-1580℃ for ladle casting; feeding wire after re-adjusting the temperature is conducive to improving the recovery rate of Mg and Re;
[0038] Casting: In the previous step, the molten steel is continuously cast to obtain a steel billet;
[0039] Rolling: After the steel billet is heated and kept warm in the previous step, it is rolled by a high-speed wire mill. The rolling specifications are Φ5.5mm-30mm, including 6 rough rolling, 12 intermediate rolling, 6 pre-finishing rolling, 10 finishing rolling, wire drawing, cooling, and the rolling passes are selected according to the size of the specifications. After the rough rolling, an "induction heating" device is installed to provide online temperature compensation for the billet.
[0040] Solution treatment: After rolling, the stainless steel material is solution treated to obtain high-end free-cutting stainless steel for precision mechanical parts.
[0041] Preferably, during LF refining, pure magnesium wire is fed first and then rare earth wire is fed immediately. Rare earth has a stronger affinity with oxygen and sulfur. Feeding magnesium wire first does not affect the effect of magnesium. To ensure the recovery rate of magnesium and rare earth, the active oxygen in the molten steel should be controlled to be ≤30ppm before wire feeding. Too high active oxygen will cause magnesium to combine with oxygen and enter the slag, which will not achieve the purpose of reforming oxidized inclusions such as Al2O3. The wire feeding speed is controlled at 140-160m / min, and the distance between the wire feeding pipe outlet and the liquid surface is controlled at 30-50cm. After wire feeding, weak stirring with argon is used, and the time is controlled at 5-8min.
[0042] Preferably, during the continuous casting process, the superheat is controlled at 25-45°C, the casting speed is controlled at 0.8-1.2 m / min, and the water flow rate of the crystallizer is 90-95 m 3 / h, foot roller water flow 2.0-2.5m 3 / h, water flow rate of secondary cooling section 2.5-3.0m 3 / h, the crystallizer adopts fast cooling, and the foot roller and the second cooling section adopt slow cooling, which is conducive to a more uniform formation of sulfides.
[0043] Preferably, before rolling, heating is carried out in three stages, namely, low temperature zone, medium temperature zone and high temperature zone, wherein the low temperature zone: temperature 850-900℃, time 50-80min; medium temperature zone: temperature 1050-1100℃, time 50-80min; high temperature zone: temperature 1230-1260℃, time 40-50min; during the rolling process, the starting temperature is required to be 1200-1250℃, and the head is rolled away from water during the entire rolling process, which can effectively prevent "head splitting". The induction heating temperature is set to 1150-1170℃ for heating the rolled piece, and after rolling, the Stelmor air cooling line controls the cooling rate to 5-10℃ / s.
[0044] Preferably, in the solution process, the wire rod is heated in two stages. First, it enters the low temperature zone at a temperature of 1000±10°C for 50 to 70 minutes, then enters the high temperature zone at a temperature of 1060±10°C for 50-60 minutes, and finally comes out of the furnace and directly enters water to cool to below 300°C.
[0045] Compared with the prior art, the high-end free-cutting stainless steel for precision mechanical parts and the preparation method thereof described in the present invention have the following significant beneficial effects:
[0046] 1. It has excellent corrosion resistance. It can keep rust-free for 240 hours in the salt spray test, which is better than sulfur-containing 316L and similar to conventional sulfur-free 316L;
[0047] 2. It has good turning performance and lower cutting force, which is better than sulfur-containing 316L and sulfur-free 316L;
[0048] 3. More importantly, the surface of the material is smooth and has no pits after processing and polishing, which is better than sulfur-containing 316L and similar to sulfur-free 316L;
[0049] 4. The high-end free-cutting stainless steel produced by the present invention has a high yield rate, which can reach more than 90%;
[0050] Therefore, the free-cutting stainless steel obtained by the present invention has excellent corrosion resistance and good turning performance through reasonable component ratio design and inclusion modification. More importantly, the surface of the material is smooth and has no pits after processing and polishing, which is suitable for making various complex parts with requirements for corrosion resistance and surface aesthetics, such as watch crowns, mobile phone lens gaskets, etc., mainly accessories, electronic and mechanical products. And the high-end free-cutting stainless steel produced by the preparation method provided by the present invention has a high yield rate, which can reach more than 90%. It has broad prospects for industrial large-scale production and market application. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is the metallographic sulfide distribution of the continuous casting billet in Example 1 of the present invention.
[0052] Figure 2 Metallographic sulfide distribution of free-cutting 316L continuous casting billet.
[0053] Figure 3 This is the metallographic sulfide distribution of the continuous casting billet in comparative example 6.
[0054] Figure 4 This is the metallographic sulfide distribution of the rolled material in Example 1 of the present invention.
[0055] Figure 5 Metallographic sulfide distribution of free-cutting 316L rolled product.
[0056] Figure 6 This is the metallographic sulfide distribution of the rolled material in Comparative Example 7.
[0057] Figure 7 This is an enlarged picture of the polished surface of the product made in Example 1 of the present invention.
[0058] Figure 8 This is an enlarged picture of the polished surface of the product made of free-cutting 316L.
[0059] Fig. 9 This is an enlarged picture of the polished surface of the product made in Comparative Example 5. DETAILED DESCRIPTION
[0060] In order to better clarify and understand the purpose, process scheme and advantages of the present invention, the technical scheme and implementation method of the present invention are further described clearly, completely and in detail through specific examples and in combination with the accompanying drawings. It should be noted that the embodiments described in the present invention are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given, but they are only part of the embodiments of the present invention, not all of the embodiments. The specific implementation methods described are limited to explaining and interpreting the present invention, and do not limit the present invention. Based on the embodiments in the present invention, all other implementation methods obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0061] The experimental methods and conditions used in the following examples are conventional methods and conventional conditions unless otherwise specified, and the materials, reagents or instruments used in the examples, unless otherwise specified, can be obtained from commercial sources. The reaction conditions embodied in the content of the invention of the present invention can achieve the reaction and obtain the product of the expected effect. Due to space limitations, only some embodiments are listed below to further illustrate the advantages of the technical solution of the present invention.
[0062] Example 1
[0063] The high-end free-cutting stainless steel for precision mechanical parts is obtained through electric furnace smelting, AOD smelting, LF refining, casting, rolling and solid solution.
[0064] Electric furnace smelting: Use scrap stainless steel with a phosphorus content of 0.030% to melt into 31 tons of crude molten steel. After the smelting, add 250 kg of ferrosilicon per ton of molten steel for reduction. After the reduction, remove all the slag and add 180 kg of carbonized rice husk for heat preservation before tapping. The tapping temperature is 1630°C.
[0065] AOD smelting: firstly, oxygen decarburization process is carried out, high temperature carbon blowing is adopted, temperature is controlled at 1690-1750℃, time is controlled at 39min, slag basicity is controlled at 3.1, and decarburization end point C is 0.004%; secondly, reduction process is carried out, 950Kg of ferrosilicon is added to molten steel, temperature is controlled at 1600-1680℃, time is controlled at 10min, and slag basicity is controlled at 1.8; refining process is carried out again, 40Kg of pure aluminum ingot is added during refining, deep deoxidation is carried out, oxygen content in steel is 21ppm at the end of refining, refining time is 11min, temperature is 1600-1650℃, slag basicity is 1.9, and sufficient ferrosulphide is added at one time according to the amount of molten steel in the later stage of refining, and the S content of molten steel is 0.15%; finally, the temperature is adjusted to 1610℃, and the molten steel is removed for the next step;
[0066] LF refining: After the molten steel arrives at the station, the temperature is measured and sampled, and the temperature is adjusted to 1640℃. According to the current stainless steel structure, 50Kg of ferrochrome, 10Kg of ferronickel, 5Kg of ferrosilicon, 20Kg of pure manganese and 20Kg of ferrosulphur are added to adjust the elements except Mg and Re to meet the requirements of their respective components. Then the temperature of the molten steel is readjusted to 1620℃. At this time, the oxygen content in the steel is 23PPm. Pure magnesium wire and rare earth wire are fed first, and the pure magnesium wire is fed immediately followed by the rare earth wire. The feeding speed is controlled at 150m / min, and the distance between the outlet of the feeding pipe and the liquid surface is controlled at 41cm. After the feeding is completed, argon is used for weak stirring for 7min. The measured Mg of the molten steel is 0.0012%, and Re is 0.0070%. Then the temperature is adjusted to 1570℃ for ladle casting.
[0067] Casting: The molten steel is continuously cast in the previous step, the superheat is controlled at 25-45℃, the casting speed is controlled at 1.1m / min, and the water flow rate of the crystallizer is 93m 3 / h, foot roller water flow 2.2m 3 / h, secondary cooling water flow 2.9m 3 / h;
[0068] Rolling: After the steel billet is heated and kept warm in the previous step, it is taken out of the furnace and rolled by the high-speed wire unit. Before rolling, it is heated in three stages. The temperature in the low-temperature zone is 850-900℃, and the heating time is 70min; the temperature in the medium-temperature zone is 1050-1100℃, and the heating time is 66min; the temperature in the high-temperature zone is 1230-1260℃, and the heating time is 46min. The rolling specification is Φ12mm, which includes 6 rough rolling, 12 intermediate rolling, 6 pre-finishing rolling, 4 finishing rolling, wire drawing, and cooling. The starting rolling temperature is 1245℃. The head is water-proof during the entire rolling process, which can effectively prevent "head splitting". The induction heating temperature is set to 1150℃ for the heated rolled piece. After rolling, the cooling rate of the Stellmore air-cooled line is 5℃ / S.
[0069] Solution treatment: The wire rod is heated in two stages. The low temperature zone is heated at 1000±10℃ for 58 minutes, and the high temperature zone is heated at 1060±10℃ for 55 minutes. Finally, it is taken out of the furnace and directly cooled in water to 25℃ to obtain high-end free-cutting stainless steel for precision mechanical parts.
[0070] The final composition of the obtained stainless steel is shown in Table 1, and the yield and mechanical properties are shown in Table 3.
[0071] The specific operations of Examples 2 to 8 are similar to those of Example 1, and the process operating parameters are slightly different within the specification range of the method of the present invention. The specific parameters are shown in Table 2. The specific components obtained in Examples 2 to 8 are shown in Table 1, and the yield and performance are shown in Table 3.
[0072] Table 1 Summary of ingredients / % of each embodiment and comparative example
[0073]
[0074]
[0075] Table 2 Process parameters of each embodiment
[0076]
[0077]
[0078]
[0079] Table 3 Summary of yield and mechanical properties of various embodiments and comparative examples
[0080]
[0081] The mechanical properties test is carried out in accordance with the standard "GB / T 228.1-2021 Metallic Materials Tensile Test Part 1_Room Temperature Test Method"; the hardness test is carried out in accordance with the standard "GB / T 231.1-2018 Metallic Materials Brinell Hardness Test Part 1: Test Method".
[0082] In order to further reflect the effect of adding Mg and Re on the machinability, corrosion resistance and surface finish after polishing of 316L stainless steel, the present invention illustrates a total of 8 embodiments and 8 comparative examples. Embodiments 1 to 8 are cases manufactured according to the method of the present invention. The contents and manufacturing parameters of the embodiments fluctuate within the scope of the invention method, as shown in Tables 1-3. The specific components of Comparative Examples 1-8 are shown in Table 1. The preparation method is basically the same as that of Example 1 and will not be repeated. The main components C, Si, Mn, P, S, Cr, Ni, Cu, Mo, and N are similar to those of the examples. The main difference is that Comparative Example 1 only adds Mg element but not Re; Comparative Example 2 only adds Re element but not Mg, and Comparative Example 3 adds Re and Mg elements at the same time, but both are lower than the design value requirements; Comparative Example 4 adds Re and Mg elements at the same time, but both are higher than the design value requirements; Comparative Example 5 adds Re and Mg elements at the same time, Mg is lower than the design value requirements, and Re is higher than the design value requirements; Comparative Example 6 adds Re and Mg elements at the same time, Mg is higher than the design value requirements, and Re is lower than the design value requirements; Comparative Example 7 only adds Mg element, but adds other elements Ca; Comparative Example 7 only adds Re element, but adds other elements Sn. Free-cutting 316L only adds free-cutting element S, without adding Mg and Re, and the other elements are similar; the difference between conventional 316L and the composition of the present invention is that conventional 316L does not add any free-cutting elements and belongs to non-free-cutting steel.
[0083] As can be seen from Table 3, when the DFW of Examples 1 to 4 and 7 is controlled at 1 to 7, the yield rate can reach more than 90%, and when the DFW of Examples 1, 2, 3, and 7 is controlled at 1.5-7.0, the yield rate is all above 94%. The DFW of Examples 5, 6, and 8 is lower than 1 or higher than 7.0, and the yield rate is relatively low, indicating that the method of the present invention controls the DFW content to specifically improve the yield rate. The mechanical properties (tensile strength, yield strength, elongation after fracture, and cross-sectional shrinkage) and hardness of Examples 1 to 8, Comparative Examples 1-8, free-cutting 316L, and conventional 316L are relatively small, and there is no regularity to be found, indicating that the stainless steel of the present invention does not have an adverse effect on strength and plasticity.
[0084] The high-end free-cutting stainless steel, comparative examples 1-8, free-cutting 316L and sulfur-free conventional 316L for precision mechanical parts produced by the present invention are simultaneously subjected to turning experiments. The turning parameters of the materials are the same. The turning experiments are carried out on the M06J lathe. The tool head is equipped with a 9129AA dynamometer. The length of the experimental material is 500mm each. The tool adopts a carbide tool, the cutting depth is 0.5mm, the feed rate is 0.15mm / r, and the cutting speed is 100m / min respectively. After continuous turning for 30min, comparative analysis is performed. The results are shown in Table 4. It can be seen that the cutting force of Examples 1-8 of the present invention is relatively low and the tool wear is smaller. The cutting force of Comparative Examples 1-8 and free-cutting 316L is higher and the tool wear is greater, while the cutting force of conventional 316L is the highest and the tool wear is the largest, indicating that the turning performance of Comparative Examples 1-8 is similar to that of free-cutting 316L, and does not play a role in further improving the turning performance. The turning performance of Examples 1-8 of the present invention is further improved on the basis of free-cutting 316L.
[0085] Table 4 Turning performance evaluation parameters
[0086]
[0087]
[0088] The corrosion resistance test experiment was carried out according to the standard "GB / T 10125-2012" "Artificial Atmosphere Corrosion Test". The results are shown in Table 5. After 240 hours, the free-cutting 316L was severely corroded, while Examples 1-8 and conventional sulfur-free 316L were not rusted, and Comparative Examples 1-8 also had slight rust. This shows that Examples 1-8 improved the corrosion resistance on the basis of free-cutting 316L, which was similar to conventional sulfur-free 316L. Comparative Examples 1-8 also slightly improved the corrosion resistance on the basis of free-cutting 316L, but did not achieve the expected effect.
[0089] Table 5 Salt spray test results and mechanical polishing surface conditions
[0090]
[0091]
[0092] Figure 1 , Figure 2 , Figure 3 They are metallographic pictures of sulfides of continuous casting billets of Example 1, free-cutting 316L and Comparative Example 6. In Example 1, the cast sulfides are dispersed in the material in granular form, mainly Type I sulfides, while most of the sulfides of free-cutting 316L and Comparative Example 6 are clustered and unevenly distributed, mainly Type II sulfides. It is generally believed in the art that Type I sulfides are beneficial to improving machinability and corrosion resistance, while Type II sulfides are detrimental to machinability and corrosion resistance.
[0093] Figure 4 , Figure 5 , Figure 6 The metallographic sulfide distributions of the rolled materials are shown in Example 1, free-cutting 316L and Comparative Example 7 respectively. Due to the modification of Mg and Re, the sulfides of Example 1 are evenly distributed in short strips after rolling, which is beneficial to turning performance. The sulfur-containing 316L and Comparative Example 7 are unevenly distributed in thin and long strips, which are not conducive to turning and are not corrosion-resistant.
[0094] Figure 7 , Figure 8 , Fig. 9 The surfaces of the products made of Example 1, free-cutting 316L and Comparative Example 5 after polishing are shown. The surface of Example 1 is smooth and has no pits, while the surfaces of free-cutting 316L and Comparative Example 5 have pits, which affect the appearance and corrosion resistance. This is the result of the influence of unmodified oxide inclusions such as Al2O3.
[0095] In short, the high-end free-cutting stainless steel for precision machinery parts produced by the present invention has good turning performance, which is better than the traditional free-cutting stainless steel with only S added; it has excellent corrosion resistance, which is better than the traditional free-cutting stainless steel with only S added, and the corrosion resistance is similar to that of non-free-cutting stainless steel 316L; more importantly, the surface of the material is smooth and has no pits after processing and polishing, which is better than the traditional free-cutting stainless steel with only S added, and is suitable for making various complex parts with requirements for corrosion resistance and surface aesthetics, such as watch crowns, mobile phone lens washers, etc., mainly accessories, electronic and mechanical products. The free-cutting steel produced by the production method of the present invention has a high yield rate, which is ≥90% or even higher, is suitable for industrial large-scale production, and has a high economic advantage.
[0096] The above-described embodiments are only preferred solutions of the present invention and are not intended to limit the present invention in any form. Other variations and modifications are possible without exceeding the technical solutions described in the claims.
Claims
1. A high-end free-cutting stainless steel for precision mechanical parts, characterized in that: The chemical composition of the stainless steel includes, by mass percentage, C≤0.03%; Si 0.2%-1.0%; Mn 1.0%-2.0%; P≤0.05%; S 0.08%-0.18%; Ni 12.0%-14.0%; Cr 16.0%-18.0%; Cu0.20%-0.60%; Mo 2.0%-3.0%; N0.02%-0.1%; Mg 0.0004%-0.006%; Re0.001%-0.010%, and the rest is Fe and unavoidable impurities.
2. According to claim 1, the high-end free-cutting stainless steel for precision machinery parts is characterized in that: The chemical composition of the stainless steel includes, by mass percentage, C≤0.028%, Si0.3-0.8%, Mn 1.2-1.8%, P≤0.045%, S 0.09-0.12%, Ni 12.3-13.0%, Cr16.5-17.5%, Cu 0.30%-0.50%, Mo 2.3%-2.8%, N 0.02%-0.08%, Mg0.0006%-0.005%, Re 0.002%-0.008%, and the rest is iron and unavoidable impurities.
3. The high-end free-cutting stainless steel for precision mechanical parts according to claim 1, characterized in that: Adjust the chemical composition to meet DFW of 1 to 7.
4. A method for preparing high-end free-cutting stainless steel for precision machinery parts according to any one of claims 1 to 3, characterized in that: The raw materials are smelted, cast, rolled and heat treated to obtain the high-end free-cutting stainless steel.
5. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: The smelting process includes electric furnace smelting, AOD smelting, and LF refining; continuous casting is used for casting; high-speed wire rolling units are used for rolling; and an annular solid solution furnace is used for solid solution.
6. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: The oxygen content in the AOD smelting process is controlled to be ≤30ppm.
7. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: During the LF refining process, after adjusting the elements other than Mg and Re in the molten steel to meet the composition requirements, the iron core wire containing magnesium powder and rare earth is fed to adjust the Mg and Re contents of the molten steel to reach the target values.
8. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: Before rolling, it is heated in three stages, namely low temperature zone, medium temperature zone and high temperature zone. The low temperature zone: temperature 850-900℃, time 50-80min; medium temperature zone: temperature 1050-1100℃, time 50-80min; high temperature zone: temperature 1230-1260℃, time 40-50min.
9. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: During the rolling process, the starting temperature is required to be 1200-1250℃.
10. The method for preparing high-end free-cutting stainless steel for precision machinery parts according to claim 4, characterized in that: The rolling process is also provided with an induction heating step, and the induction heating is set to heat the rolled piece to a temperature of 1150-1170°C.
Citation Information
Patent Citations
Selenium-containing and calcium-containing free-cutting stainless steel and preparation method thereof
CN115466908A
Free-cutting martensitic stainless steel subjected to tellurium-magnesium composite treatment and preparation method thereof
CN116676530A
Non-magnetic stainless steel having excellent cold forgeability and hydrogen embrittlement resistance or corrosion resistance