Hot-dip plated steel material
By controlling the random orientation of MgZn2 phase and α phase in the plating layer of hot-dip plating steel, and combining specific chemical composition, the problems of taking into account both plane corrosion resistance and replacement corrosion resistance are solved, and the efficient corrosion resistance of the plating is achieved. Corrosion-proof.
Patent Information
- Application Number
- CN202411119441.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-20
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-22
AI Technical Summary
Existing hot-dip plating steels are difficult to take into account both the plane corrosion resistance and the alternative corrosion resistance, and there is a lack of effective technical solutions.
By controlling the crystal orientation of the MgZn2 phase and the α phase in the hot-dip plating layer, they are oriented in a random direction, and combining specific chemical compositions such as Al: 10.0-30.0%, Mg: 3.0-15.0%, Fe: 0.01-15.0% The content of equal elements and through the X-ray diffraction intensity relationship (such as 0.5≤I(100)MgZn2/{I(002)MgZn2+I(101)MgZn2}≤2.5 and 0.2≤I(111)α/I(200) α≤5.0), ensures excellent planar corrosion resistance and replacement corrosion resistance of the coating.
The significant improvement in the plane corrosion resistance and replacement corrosion resistance of hot-dip plating steel has been achieved, ensuring that the plating uniformly generates corrosion products during the corrosion process, and improving the overall performance of the plating.
Smart Images

Figure CN118996307A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 202380011131.7, which entered the Chinese national phase based on PCT / JP2023 / 013666 with an application date of March 31, 2023. Technical Field
[0002] The present invention relates to hot-dip galvanized steel products.
[0003] This application claims priority based on Japanese Patent Application No. 2022-069530 filed in Japan on April 20, 2022, and the contents are incorporated herein by reference. Background Art
[0004] Steel materials with a hot-dip Zn-plated layer containing Al and Mg formed on the surface (hot-dip Zn-Al-Mg-plated steel materials) have excellent corrosion resistance. Therefore, hot-dip Zn-Al-Mg-plated steel materials are widely used as materials for structural members requiring corrosion resistance, such as building materials.
[0005] For example, Patent Document 1 describes a hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer formed on the surface of the steel sheet, wherein the hot-dip plated layer contains, in average composition, 0 to 90% by mass of Al and 0 to 10% by mass of Mg, and the remainder contains Zn and impurities, and a pattern (layout) portion and a non-pattern portion arranged in a manner to form a prescribed shape are formed in the hot-dip plated layer, the pattern portion and the non-pattern portion respectively contain one or two of a first region and a second region, the absolute value of the difference between the area ratio of the first region in the pattern portion and the area ratio of the first region in the non-pattern portion is greater than 30%, the first region is a region having an orientation ratio of greater than 3.5, and the second region is a region having an orientation ratio of less than 3.5.
[0006] Patent document 2 describes a Zn-Al-Mg hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer, wherein the hot-dip plated layer contains 4 mass % to 22 mass % of Al and 1 mass % to 5 mass % of Mg, and the remainder comprises Zn and unavoidable impurities, and the ratio of the X-ray diffraction intensity I(200) of the (200) plane of the Al phase in a cross section of the hot-dip plated layer parallel to the surface of the hot-dip plated layer to the X-ray diffraction intensity I(111) of the (111) plane of the Al phase, i.e., the diffraction intensity ratio I(200) / I(111) is greater than 0.8.
[0007] In recent years, hot-dip galvanized steel materials used as building materials such as roofs and wall materials have been required to have a high level of compatibility between the corrosion resistance of the coating itself, i.e., flat corrosion resistance, and the alternative corrosion resistance for protecting the base metal from corrosion when the base metal is exposed. In the prior art, there has been little research on the compatibility between flat corrosion resistance and alternative corrosion resistance.
[0008] Patent Document 1 shows that the diffraction peak intensity I of the (0002) plane of the Zn phase 0002 The diffraction peak intensity I 10-11 When the area with an intensity ratio of 3.5 or more is set as the first area, and the area with an intensity ratio of less than 3.5 is set as the second area, the difference between the area ratio of the first area in the pattern part and the area ratio of the first area in the non-pattern part is set to more than 30%, so that text, design, etc. can appear intentionally on the surface of the coating, but the alternative corrosion resistance has not been studied.
[0009] In Patent Document 2, although the appearance of the plated layer is set to a fine-textured, smooth, pear-skin appearance with many glossy portions by controlling the orientation of the Al phase in the plated layer, no study is made on the chemical corrosion resistance.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2021-85086
[0013] Patent Document 2: International Publication No. 2011 / 001662 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a hot-dip plated steel material having both excellent flat corrosion resistance and chemical corrosion resistance.
[0016] Means for solving problems
[0017] In order to solve the above-mentioned problems, the present invention adopts the following configuration.
[0018] [1] A hot-dip galvanized steel material comprising:
[0019] steel; and
[0020] The hot-dip coating is disposed on the surface of the steel material.
[0021] The chemical composition of the hot-dip coating contains, by mass %, the following:
[0022] Al: 10.0-30.0%,
[0023] Mg: 3.0-15.0%,
[0024] Fe: 0.01~15.0%,
[0025] Si: 0-10.0%,
[0026] Ni: 0-1.0%,
[0027] Ca: 0-4.0%,
[0028] further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less,
[0029] The rest: contains Zn and impurities,
[0030] The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship of the following formula (1a) and formula (2a).
[0031] 0.5≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2}≤2.5(1a)
[0032] 0.2≤I(111) α / I(200) α ≤5.0(2a)
[0033] Where, I(100) in formula (1a) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0034] [2] A hot-dip galvanized steel material comprising:
[0035] steel; and
[0036] The hot-dip coating is disposed on the surface of the steel material.
[0037] The chemical composition of the hot-dip coating contains, by mass %, the following:
[0038] Al: 15.0-30.0%,
[0039] Mg: 5.0-10.0%,
[0040] Fe: 0.01~15.0%,
[0041] Si: 0-10.0%,
[0042] Ni: 0-1.0%,
[0043] Ca: 0-4.0%,
[0044] further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less,
[0045] The rest: contains Zn and impurities,
[0046] The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship of the following formula (1b) and formula (2b).
[0047] 1.0≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2}≤2.0(1b)
[0048] 0.2≤I(111) α / I(200) α ≤5.0(2b)
[0049] Where, I(100) in formula (1b) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2b) αis the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0050] [3] The hot-dip plated steel material according to [1] or [2], wherein the Sn content in the chemical composition of the hot-dip plated layer is set to 0.05 to 0.5% by mass,
[0051] The Mg2Sn phase was detected from the X-ray diffraction measurement results of the hot-dip galvanized layer.
[0052] Effects of the Invention
[0053] According to the above aspects of the present invention, it is possible to provide a hot-dip plated steel material having both excellent flat corrosion resistance and excellent chemical corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 It is a schematic cross-sectional view of a hot-dip plated steel material as an embodiment of the present invention. DETAILED DESCRIPTION
[0055] The chemical corrosion resistance of the coating is achieved by forming a coating containing an element (such as Zn, Mg, etc.) with a higher ionization tendency than the base metal on the surface of the steel material, so that the coating corrodes preferentially relative to the base metal. Therefore, the improvement of chemical corrosion resistance brought about by the coating is not compatible with the improvement of the corrosion resistance of the coating itself, that is, the improvement of the plane corrosion resistance.
[0056] Therefore, the inventors of the present invention have conducted in-depth research to improve both the flat corrosion resistance and the chemical corrosion resistance of the hot-dip Zn-plated layer containing Al and Mg. The MgZn2 phase and the α phase contained in the coating layer each contain various crystal orientation planes. The corrosion resistance of these crystal orientation planes is not the same in all orientation planes. For example, the corrosion resistance of the crystal orientation plane that becomes a dense plane is relatively high, but on the other hand, the corrosion resistance of the crystal orientation plane other than the dense plane becomes relatively low.
[0057] Therefore, in order to achieve the above-mentioned purpose, the inventors of the present invention have tried to orient the crystal orientation of the MgZn2 phase and the α phase contained in the coating in a random direction for each grain. Such a coating becomes a mixture of crystal orientation planes with various orientations of different corrosion resistance on its surface. If such a coating is corroded, the crystal orientation plane with relatively low corrosion resistance will be corroded first, and then the crystal orientation plane with relatively high corrosion resistance will be corroded. As a result, the corrosion of the MgZn2 phase and the α phase is carried out in a balanced manner, and the dissolution of Zn ions and Mg ions is continued for a long time, so that the chemical corrosion resistance can be ensured. In addition, it is found that: by the balanced corrosion of the MgZn2 phase and the α phase, the corrosion products are generated more evenly on the surface of the coating, and the barrier function is maintained by the moderate survival of the α phase, thereby improving the plane corrosion resistance.
[0058] Therefore, it was discovered that when the X-ray diffraction intensity obtained from the X-ray diffraction measurement results for the coating surface satisfies the relationship between the following formula (1a) and the following formula (2), the crystal orientation of the MgZn2 phase and the α phase is oriented in a random direction for each grain, which can improve both the planar corrosion resistance and the chemical corrosion resistance, thereby completing the present invention.
[0059] The hot-dip plated steel material as an embodiment of the present invention is described below. The hot-dip plated steel material of the present embodiment is the following hot-dip plated steel material: it has a steel material and a hot-dip plated layer arranged on the surface of the steel material, and the chemical composition of the hot-dip plated layer contains, by mass%, Al: 10.0-30.0%, Mg: 3.0-15.0%, Fe: 0.01-15.0%, Si: 0-10.0%, Ni: 0-1.0%, Ca: 0-4.0%, and further contains Sb: 0-0.5%, Pb: 0-0.5%, Cu: 0-1.0%, Sn: 0-2.0%, Ti: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mn: 0-1.0% , Mo: 0~1.0%, Ag: 0~1.0%, Li: 0~1.0%, La: 0~0.5%, Ce: 0~0.5%, B: 0~0.5%, Y: 0~0.5%, P: 0~0.5%, Sr: 0~0.5%, Co: 0~0.5%, Bi: 0~0.5%, In: 0~0.5%, V: 0~0.5%, W: 0~0.5%, and the total amount of these elements is set to 5% or less, and the remainder: contains Zn and impurities, and the diffraction intensity of the hot-dip galvanized layer obtained by the X-ray diffraction measurement result satisfies the relationship between the following formulas (1a) and (2).
[0060] 0.5≤I(100) MgZn2 / {I(002) MgZn2+I(101) MgZn2}≤2.5(1a)
[0061] 0.2≤I(111) α / I(200) α ≤5.0 (2)
[0062] Where, I(100) in formula (1a) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of MgZn2 phase, I(111) in formula (2) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0063] In addition, when the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, it is preferable to satisfy the above formula (2) and the following formula (1b) instead of the above formula (1a). It should be noted that when the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, and satisfy the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, it is sufficient to satisfy the above formula (1a). When the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, and satisfy the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, respectively, it is preferable to satisfy the above formula (1a), and it is more preferable to satisfy the following formula (1b).
[0064] 1.0≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2}≤2.0(1b)
[0065] In the following description, the "%" expression of the content of each element in the chemical composition means "mass %". The content of the elements in the chemical composition is sometimes recorded as element concentration (for example, Zn concentration, Mg concentration, etc.). "Flat surface corrosion resistance" refers to the property of the hot-dip galvanizing layer (specifically, the Zn-Al-Mg alloy layer) itself that is not easy to corrode. "Chemical corrosion resistance" refers to the property of inhibiting corrosion of steel at the exposed parts of the steel (for example, the cut end surface of the plated steel, the cracked part of the hot-dip galvanizing layer during processing, and the part where the steel is exposed due to the peeling of the hot-dip galvanizing layer). "Hot-dip galvanizing layer" refers to a plating film produced by the so-called hot-dip galvanizing process.
[0066] like Figure 1 As shown in , the hot-dip galvanized steel material 1 of this embodiment has a steel material 11. There is no particular limitation on the shape of the steel material 11, and an example of the steel material 11 is a steel plate. In addition, the steel material 11 may also be a steel pipe, civil engineering and construction materials (fences, corrugated pipes, gutter covers, sand-proof plates, bolts, wire meshes, guardrails, water-blocking walls, etc.), home appliance components (housings of outdoor units of air conditioners, etc.), automobile parts (travel components, etc.) and other base steel materials that have been formed. Forming processing includes, for example, various plastic processing methods such as pressing, roll forming, and bending.
[0067] There is no particular restriction on the material of the steel material 11. The steel material 11 can be, for example, ordinary steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steel containing strengthening elements such as Ni and Cr). The steel material 11 can also be a hot-rolled steel sheet, hot-rolled steel strip, cold-rolled steel sheet, and cold-rolled steel strip described in JIS G 3302: 2010. There is no particular restriction on the manufacturing method of the steel sheet (hot rolling method, pickling method, cold rolling method, etc.) and its specific manufacturing conditions.
[0068] As described below, for the steel material to be the plated original plate, a pre-plated steel material in which the surface of the steel material 11 is pre-plated is used. An example of the pre-plated steel material is a pre-Ni plated steel material having a Ni plating layer formed on the surface of the steel material 11. The pre-plated steel material can be obtained, for example, by electrolytic treatment or displacement plating. The electrolytic treatment is carried out by immersing the base steel material in a sulfuric acid bath or a chloride bath containing metal ions of various pre-plating components and performing an electrolytic treatment. The displacement plating is carried out by immersing the base steel material in an aqueous solution containing metal ions of various pre-plating components and having its pH adjusted with sulfuric acid to cause metal displacement precipitation.
[0069] The hot-dip plated steel material 1 of the present embodiment has a hot-dip coating 12 disposed on the surface of the steel material 11. The hot-dip coating 12 of the hot-dip plated steel material 1 of the present embodiment is caused by the chemical composition described later and is mainly composed of a Zn-Al-Mg alloy layer. In addition, the hot-dip coating 12 of the hot-dip plated steel material 1 of the present embodiment may also include an interface alloy layer between the steel material 11 and the Zn-Al-Mg alloy layer. That is, the hot-dip coating 12 may be a single-layer structure of the Zn-Al-Mg alloy layer, or a laminated structure including the Zn-Al-Mg alloy layer and the interface alloy layer. The interface alloy layer may also include an Al-Ni alloy phase. The Al-Ni alloy phase is derived from an Al-Ni compound formed by the reaction of Ni of the Ni coating of the pre-plated steel material with Al of the hot-dip coating bath as described below. In the hot-dip plated steel material 1, an interface alloy layer including an Al-Ni alloy phase may also be formed in the entire interface between the steel material 1 and the hot-dip coating 12. Alternatively, an interface alloy layer including an Al—Ni alloy phase may be formed in a portion of the interface, and an interface alloy layer including a Fe—Al alloy phase may be formed in the other portion.
[0070] The chemical composition of the hot-dip coating of the present embodiment is composed of Zn and other alloying elements. The chemical composition of the hot-dip coating is described in detail below. It should be noted that the elements whose lower limit of concentration is described as 0% are not necessary to solve the problem of the hot-dip coated steel material of the present embodiment, but are optional elements that are allowed to be included in the hot-dip coating for the purpose of improving properties.
[0071] <Al:10.0~30.0%>
[0072] Al forms a solid solution with Zn, namely, the α phase, which helps to improve the corrosion resistance of the flat part, the chemical corrosion resistance and the processability. Therefore, the Al concentration is set to 10.0% or more. The Al concentration can also be set to 11.0% or more, 12.0% or more, or 15.0% or more. On the other hand, when Al is excessive, the Mg concentration and the Zn concentration are relatively reduced, and the chemical corrosion resistance deteriorates. Therefore, the Al concentration is set to 30.0% or less. The Al concentration can also be set to 28.0% or less, 25.0% or less, or 20.0% or less.
[0073] <Mg:3.0~15.0%>
[0074] Mg is an element necessary to ensure the corrosion resistance of the planar portion and the chemical corrosion resistance. Therefore, the Mg concentration is set to 3.0% or more. The Mg concentration can also be set to 4.0% or more, 5.0% or more, or 6.0% or more. On the other hand, if the Mg concentration is excessive, the processability, especially the powdering property, may deteriorate, and the corrosion resistance of the planar portion may deteriorate. Therefore, the Mg concentration is set to 15.0% or less. The Mg concentration can also be set to 12.0% or less, 10.0% or less, or 8.0% or less.
[0075] <Fe:0.01%~15.0%>
[0076] The concentration of Fe may also be 0%. On the other hand, the hot-dip coating may contain 0.01% or more of Fe. It has been confirmed that if the Fe concentration is 15.0% or less, there is no adverse effect on the performance of the hot-dip coating. The Fe concentration may also be set to, for example, 0.05% or more, 0.1% or more, 0.5% or more, or 1.0% or more. The Fe concentration may also be set to, for example, 10.0% or less, 8.0% or less, or 6.0% or less. Fe may be mixed in from the base steel plate, so the Fe concentration may also be 0.05% or more.
[0077] <Si:0%~10.0%>
[0078] The Si concentration may also be 0%. On the other hand, Si contributes to the improvement of the corrosion resistance of the planar portion. Therefore, the Si concentration may be set to 0.05% or more, 0.1% or more, 0.2% or more, or 0.5% or more. On the other hand, if the Si concentration is excessive, the corrosion resistance of the planar portion and the chemical corrosion resistance deteriorate. Therefore, the Si concentration is set to 10.0% or less. The Si concentration may also be set to 8.0% or less, 7.0% or less, or 6.0% or less.
[0079] <Ni:0~1.0%>
[0080] The concentration of Ni may also be 0%. On the other hand, Ni contributes to the improvement of chemical corrosion resistance. Therefore, the Ni concentration may be set to 0.05% or more, 0.08% or more, or 0.1% or more. On the other hand, if the Ni concentration is excessive, the corrosion resistance of the flat portion deteriorates. Therefore, the Ni concentration is set to 1.0% or less. The Ni concentration may also be set to 0.8% or less, 0.6% or less, or 0.5% or less.
[0081] <Ca:0%~4.0%>
[0082] The Ca concentration can also be 0%. On the other hand, Ca is an element that can adjust the Mg dissolution amount that is optimal for imparting corrosion resistance to the flat portion. Therefore, the Ca concentration can also be 0.05% or more, 0.1% or more, or 0.5% or more. On the other hand, if the Ca concentration is excessive, the corrosion resistance and workability of the flat portion deteriorate. Therefore, the Ca concentration is set to 4.0% or less. The Ca concentration can also be set to 3.5% or less, 3.0% or less, or 2.8% or less.
[0083] Furthermore, in the hot-dip coating layer of the present embodiment, it contains one or more elements from the element group of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, W: 0 to 0.5%. The total of these elements is set to 5% or less. If the total exceeds 5%, there is a possibility that the flat corrosion resistance or substitutional corrosion prevention performance decreases.
[0084] <Sb, Pb: are each 0 to 0.5% respectively>
[0085] The concentrations of Sb and Pb can also be 0%. On the other hand, Sb and Pb contribute to the improvement of substitutional corrosion prevention performance. Therefore, the concentrations of Sb and Pb can each be set to 0.05% or more, 0.10% or more, or 0.15% or more. On the other hand, if the concentrations of Sb and Pb are excessive, the corrosion resistance of the flat portion deteriorates. Therefore, the concentrations of Sb and Pb are each set to 0.5% or less. The concentrations of Sb and Pb can also be each set to 0.4% or less, 0.3% or less, or 0.25% or less.
[0086] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li: are each 0 to 1.0% respectively>
[0087] The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li can also be 0% respectively. On the other hand, they contribute to the improvement of substitutional corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li can also be set to 0.05% or more, 0.08% or more, or 0.10% or more. On the other hand, if the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li are excessive, the corrosion resistance of the planar part deteriorates. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li are set to 1.0% or less. The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li can also be set to 0.8% or less, 0.7% or less, or 0.6% or less.
[0088] <Sn: 0 to 2.0%>
[0089] The Sn concentration can also be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the substitutional corrosion resistance of the hot-dip coating. Therefore, the Sn concentration can also be set to 0.05% or more, 0.1% or more, or 0.2% or more. However, if the Sn concentration is excessive, the planar corrosion resistance deteriorates. Therefore, the Sn concentration is set to 2.0% or less. The Sn concentration can also be set to 1.5% or less, 1.0% or less, 0.6% or less, or 0.5% or less.
[0090] <La, Ce, B, Y, P, and Sr: 0 to 0.5% respectively>
[0091] The concentrations of La, Ce, B, Y, P, and Sr can also be 0% respectively. On the other hand, La, Ce, B, Y, P, and Sr contribute to the improvement of substitutional corrosion resistance. Therefore, the concentrations of La, Ce, B, Y, P, and Sr can also be set to 0.10% or more, 0.15% or more, or 0.20% or more respectively. On the other hand, if the concentrations of La, Ce, B, Y, P, and Sr are excessive, the corrosion resistance of the planar part deteriorates. Therefore, the concentrations of La, Ce, B, Y, P, and Sr are set to 0.5% or less respectively. The concentrations of La, Ce, B, Y, P, and Sr can also be set to 0.4% or less, 0.3% or less respectively.
[0092] <Co, Bi, In, V, W: 0 to 0.5% respectively>
[0093] The concentration of each of Co, Bi, In, V, and W may also be 0%. On the other hand, Co, Bi, In, V, and W contribute to the improvement of chemical corrosion resistance. Therefore, the concentration of Co, Bi, In, V, and W may be set to 0.10% or more, 0.15% or more, or 0.20% or more, respectively. On the other hand, if the concentration of Co, Bi, In, V, and W is excessive, the corrosion resistance of the planar portion deteriorates. Therefore, the concentration of Co, Bi, In, V, and W is set to 0.5% or less, respectively. The concentration of Co, Bi, In, V, and W may also be set to 0.4% or less, or 0.3% or less, respectively.
[0094] <Remainder: Zn and impurities>
[0095] The remainder of the components of the hot-dip coating of this embodiment is Zn and impurities. Zn is an element that gives the hot-dip coating flat surface corrosion resistance and chemical corrosion resistance. Impurities refer to components contained in the raw materials or components mixed in the manufacturing process, and are not intentionally contained. For example, in the hot-dip coating, sometimes due to mutual atomic diffusion between the base steel and the coating bath, components other than Fe as impurities are mixed in trace amounts.
[0096] The chemical composition of the hot-dip coating is measured by the following method. First, the hot-dip coating is stripped and dissolved using an acid containing an inhibitor that inhibits steel corrosion to obtain an acid solution. Next, the obtained acid solution is subjected to inductively coupled plasma (ICP) analysis. In this way, the chemical composition of the hot-dip coating can be obtained. The type of acid is not particularly limited as long as it can dissolve the hot-dip coating. It should be noted that the chemical composition measured by the above-mentioned means is the average chemical composition of the entire hot-dip coating.
[0097] Next, the metal structure of the hot-dip galvanized layer will be described.
[0098] The metal structure of the hot-dip coating contains α phase and MgZn2 phase. α phase and MgZn2 phase improve the corrosion resistance of the flat part of the hot-dip coating. In addition, as described below, the α phase and MgZn2 phase are randomly oriented, thereby improving the chemical corrosion resistance of the hot-dip coated steel.
[0099] The area ratio of the α phase in the hot-dip galvanized layer is preferably 15 to 80%. In addition, the area ratio of the MgZn2 phase is preferably 5 to 55%. The combined area ratio of the α phase and the MgZn2 phase is preferably 20% to 100%. However, the range of the area ratio is an example, and the area ratio of the structure of the hot-dip galvanized layer of the present invention is not limited to this range, as long as the hot-dip galvanized layer satisfies at least one of the formulas (1a) and (1b) described below and formula (2).
[0100] In addition, when the hot-dip coating contains 0.05 to 0.5% Sn, the hot-dip coating reliably contains the Mg2Sn phase. Since the Mg2Sn phase is a small amount, its presence is confirmed by X-ray diffraction measurement. By including the Mg2Sn phase in the hot-dip coating, the chemical corrosion resistance of the hot-dip coated steel is further improved.
[0101] The hot-dip coating may also contain phases other than the α phase and the MgZn2 phase as the remainder. For example, the hot-dip coating of the above chemical composition may contain η-Zn phase, Al-Ca-Si phase, etc. As long as the content of the α phase and the MgZn2 phase is within the above range, the corrosion resistance of the plane part and the chemical corrosion resistance can be ensured, so the composition of the phases or structures other than the α phase and the MgZn2 phase is not particularly limited.
[0102] Next, the crystal orientations of the α phase and the MgZn2 phase will be described.
[0103] As for the hot-dip coating of the present embodiment, when the X-ray diffraction intensity of the hot-dip coating obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2), the crystal orientation of the MgZn2 phase and the α phase is oriented in a random direction for each grain, thereby improving both the chemical corrosion resistance and the plane corrosion resistance.
[0104] 0.5≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2}≤2.5(1a)
[0105] 0.2≤I(111) α / I(200) α ≤5.0 (2)
[0106] In addition, when the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, it is preferable to satisfy the above formula (2) and the following formula (1b) instead of the above formula (1a). It should be noted that when the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, and satisfy the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, it is sufficient to satisfy the above formula (1a). When the Al concentration and Mg concentration in the chemical composition of the hot-dip coating are in the range of Al: 15.0 to 30.0% and Mg: 5.0 to 10.0%, respectively, and satisfy the range of Al: 10.0 to 30.0% and Mg: 3.0 to 15.0%, respectively, it is preferable to satisfy the above formula (1a), and it is more preferable to satisfy the following formula (1b).
[0107] 1.0≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2}≤2.0(1b)
[0108] Among them, I(100) in formula (1a) and formula (1b) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase. In addition, I(111) in formula (2) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
[0109] As shown in formula (1a), by I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2} is in the range of 0.5 to 2.5, so that the crystal orientation of the MgZn2 phase is oriented in a random direction for each grain. Preferably, in the case of an Al concentration of 15.00 to 30.00% and a Mg concentration of 5.00 to 10.00%, it is preferably in the range of 1.0 to 2.0 as shown in formula (1b). Furthermore, in I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2 When} becomes 1.06, the MgZn2 phase is oriented most randomly, so I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2} is more preferably in the range of 1.0 to 1.2.
[0110] In addition, through I(111) in formula (2) α / I(200) α The range of 0.2 to 5.0 makes the crystal orientation of the α phase random for each crystal grain. α / I(200) α When it becomes 2.1, the α phase is oriented most randomly, so I(111) α / I(200) α A more preferred range is 2.0 to 2.2.
[0111] The method for determining the area ratio of the MgZn2 phase is as follows. The surface of the hot-dip coating of a sample cut into 30 mm × 30 mm is adjusted to be flat by mechanical grinding (for example, grinding with sandpaper #2000). Then, chemical grinding is performed on the surface of the coating by colloidal grinding until the surface becomes a mirror surface. The surface of the polished coating is observed by a scanning electron microscope (SEM). Specifically, an element distribution image is taken using a scanning electron microscope-energy dispersive spectroscopy (SEM-EDS) at a magnification of 5000 times. In this element distribution image, the phase in which Mg and Zn coexist is determined to be the MgZn2 phase. It should be noted that in this specification, the region where Mg: 20 to 40 atomic % and Zn: 50 to 80 atomic % will be judged as the phase in which Mg and Zn coexist (MgZn2 phase). After the MgZn2 phase was identified, the area ratios of the α phase and the MgZn2 phase contained in the field of view were calculated by binarization using image analysis software.
[0112] The method for determining the area ratio of the α phase is as follows. The surface of the hot-dip coating of a sample cut into 30 mm × 30 mm is adjusted to be flat by mechanical grinding. Then, the surface of the coating is chemically polished by colloidal polishing until the surface becomes a mirror surface. The surface of the polished coating is observed by SEM. Specifically, an element distribution image is taken using SEM-EDS at a magnification of 5000 times. In the element distribution image, the phase in which Al and Zn coexist is determined to be the α phase. It should be noted that in this specification, the area where Al: 40 to 95 atomic % and Zn: 0.5 to 50 atomic % will be judged as the phase in which Al and Zn coexist (α phase). After determining the α phase, the area ratio of the α phase contained in the field of view is calculated by binarization using image analysis software.
[0113] I(100) in formula (1a) and formula (1b) MgZn2 / {I(002) MgZn2 +I(101) MgZn2The method for determining the} is as follows. First, the surface of the hot-dip galvanized layer is mirror-polished and chemically polished as needed. Next, an X-ray diffraction device (Rigaku Corporation (model RINT-TTR III), set the X-ray output power to 50kV, 300mA, copper target, goniometer TTR (horizontal goniometer), Kβ filter slit width to 0.05mm, length limiting slit width to 2mm, light receiving slit width to 8mm, light receiving slit 2 open, and as measurement conditions, set the scanning speed to 5 degrees / minute, step width to 0.01 degrees, and scanning axis 2θ (5~90°) to implement X-ray diffraction measurement. Then, measure the diffraction intensity of the (100) plane of the MgZn2 phase (maximum intensity within the range of 19.67±0.2°), the diffraction intensity of the (002) plane (maximum intensity within the range of 20.78±0.2°), and the diffraction intensity of the (101) plane (maximum intensity within the range of 22.26±0.2°). The diffraction intensity is set to the intensity after removing the background intensity. I(100) is calculated from the obtained diffraction intensity. MgZn2 / {I(002) MgZn2 +I(101) MgZn2}.
[0114] I(111) in formula (2) α / I(200) α The measurement method is as follows. First, the surface of the hot-dip galvanized layer is mirror-polished and chemically polished as needed. Next, for example, the X-ray diffraction apparatus and measurement conditions are set to be the same as above, and an X-ray diffraction measurement is performed. Then, the diffraction intensity of the (111) plane of the α phase (maximum intensity within the range of 38.47±0.2°) and the diffraction intensity of the (200) plane (maximum intensity within the range of 44.74±0.2°) are measured respectively. The diffraction intensity is set to the intensity after removing the background intensity. I(111) is calculated from the obtained diffraction intensity. α / I(200) α .
[0115] In addition, whether or not the hot-dip galvanized layer contains a Mg2Sn phase can be determined by whether or not a diffraction peak specific to Mg2Sn appears when performing the above-mentioned X-ray diffraction measurement.
[0116] The coating weight per single side of the hot-dip coating is set to, for example, 20 to 150 g / m 2 By setting the adhesion amount per single side to 20g / m 2 The above can further improve the flat corrosion resistance and chemical corrosion resistance of the hot-dip galvanized steel. On the other hand, by setting the adhesion amount per single side to 150g / m 2 The following can further improve the workability of the hot-dip plated steel material.
[0117] Next, a method for producing the hot-dip plated steel material of the present embodiment will be described, but the method for producing the hot-dip plated steel material of the present embodiment is not particularly limited. For example, the hot-dip plated steel material of the present embodiment can be obtained according to the production conditions described below.
[0118] In the method for manufacturing a hot-dip plated steel material of the present embodiment, a pre-Ni plated steel material in which a steel material 11 is pre-plated with Ni is used as a plated original plate. The surface of the steel material 11 is subjected to a treatment for imparting strain before the pre-Ni plating. Next, the pre-Ni plated steel material is annealed in a reducing atmosphere, and the pre-Ni plated steel material immediately after the annealing is immersed in a hot-dip plating bath and then picked up, thereby forming a hot-dip plating layer on the surface of the steel material. Next, spray cooling is performed while the temperature of the hot-dip plating layer is from the bath temperature until it becomes 300° C. or less.
[0119] First, the preparation method of the plated original plate is described. First, the surface of the steel material 11 is subjected to a treatment to impart strain. Specifically, the surface of the steel material 11 is subjected to a grinding treatment or a polishing treatment. The grinding amount in the case of the grinding treatment is not particularly limited, but for example, it can be at least 0.1 mm or more. On the other hand, regarding the polishing treatment, in order to remove the stains and oils attached to the surface of the steel material 11, for example, alkaline washing is performed, but at this time, the surface of the steel material is polished by a metal brush (grinding brush). As a result, a large number of scratches and scratches are formed on the surface of the steel material to impart strain. The amount of depression of the grinding brush during grinding is 0.5 to 10.0 mm. When the amount of depression of the grinding brush is less than 0.5 mm, sufficient strain cannot be imparted, and the α phase and the MgZn2 phase will not be randomly oriented during the process of solidifying the hot-dip coating described later. In addition, it is preferred to apply a 1.0 to 5.0% aqueous solution of NaOH on the surface of the steel plate when grinding the surface of the steel material. Thus, the dirt and oil attached to the surface of the steel material 11 are fully removed. In order to give sufficient strain to the steel plate, the pressing amount of the grinding brush used in grinding is 0.5 to 10.0 mm. The rotation speed of the grinding brush is preferably 100 to 1000 rpm. Next, the surface of the steel material 11 is plated with Ni. The adhesion amount of the Ni plating layer is set to, for example, 0.05 to 5.0 mg / m 2 . The pre-Ni plated steel is prepared in this way.
[0120] Next, the pre-Ni-plated steel is annealed in a reducing atmosphere. The annealing condition sets the soaking temperature to less than 600°C. When the soaking temperature is above 600°C, Ni and Fe are alloyed, so that the formation of Al-Ni compounds does not occur, and the number of nucleation sites is reduced so that the α phase and MgZn2 phase do not orient randomly. There is no particular restriction on the lower limit of the soaking temperature, but for example, it can also be above 500°C. A more preferred soaking temperature is above 550°C. In addition, there is no particular restriction on the soaking time, but for example, it is appropriate to set the soaking time to 0 to 2 minutes. The annealing atmosphere can be a reducing atmosphere without any particular limitation. For example, it can also be a mixed atmosphere of hydrogen and nitrogen.
[0121] The steel material immediately after annealing is immersed in a hot dip coating bath. The chemical composition of the hot dip coating bath may be appropriately adjusted so as to obtain the chemical composition of the hot dip coating layer. In addition, the temperature of the hot dip coating bath is not particularly limited, and a temperature at which hot dip coating can be performed may be appropriately selected. For example, the coating bath temperature may be set to a value that is about 20° C. higher than the melting point of the coating bath.
[0122] Next, the steel material with the molten metal attached is scooped out of the hot dip coating bath. By controlling the scooping speed of the steel material, the amount of hot dip coating attached can be controlled. If necessary, the amount of hot dip coating attached can be controlled by wiping the steel material with the hot dip coating attached. The amount of hot dip coating attached is not particularly limited, and can be set within the above range, for example.
[0123] Next, the hot-dip coating is cooled. For cooling, the steel material is spray-cooled just after being taken out of the hot-dip coating bath. Spray cooling is continuously performed while the temperature of the hot-dip coating layer is from the bath temperature to 300°C. The cooling condition below 300°C is not particularly limited, and spray cooling may be performed subsequently, or air cooling or natural cooling may be performed.
[0124] Spray cooling is performed by spraying mist water onto the surface of the hot dip coating. Spraying mist water onto the surface of the coating gives vibration to the hot dip coating. The spray volume is set, for example, to 1.0 to 30 [L / (mm 2 · minutes)], and the spray time is set to 1 to 60 seconds.
[0125] The spray volume is less than 1.0 [L / (mm 2 ·min)], the steel material will not be sufficiently vibrated, and it will be difficult for the α phase and MgZn2 phase to be randomly oriented during the solidification of the hot-dip galvanized layer. In addition, if the spray volume exceeds 30 [L / (mm 2 · minutes)], the surface of the coating will be excessively oxidized, causing poor appearance.
[0126] When the spraying time is less than 1 second, the steel material will not be sufficiently vibrated, and it becomes difficult for the α phase and the MgZn2 phase to be randomly oriented when the hot-dip coating solidifies. There is no upper limit on the spraying time, but even if it exceeds 60 seconds, the effect of the spraying is saturated, so it is set to less than 60 seconds.
[0127] By cooling the hot-dip coating layer so as to satisfy the above conditions, a hot-dip coating layer satisfying at least one of the above formula (1a) and formula (1b) and formula (2) can be formed. The reason for this is presumed to be as follows.
[0128] In the above-mentioned manufacturing method, as the plated original plate, a pre-Ni plated steel material with strain applied to the surface of the steel material in advance is used. If such a pre-Ni plated steel material is hot-dip plated, the Ni of the pre-Ni plated steel material reacts with the Al of the hot-dip bath to form Al-Ni compounds on the surface of the steel material. In addition, the strain applied to the surface of the steel material causes Al-Ni compounds to be formed in larger quantities. The Al-Ni compounds serve as nucleation sites when the coating solidifies. Furthermore, by vibrating the steel material using spray cooling after hot-dip plating, the nucleation sites are further increased. It is inferred that a large number of nucleation sites are formed by such an operation, so that when the hot-dip coating solidifies, the α phase and the MgZn2 phase become randomly oriented.
[0129] Example
[0130] The following is an explanation of the embodiments of the present invention. However, the conditions in the embodiments are only a condition example adopted to confirm the feasibility and effect of the present invention. The present invention is not limited to this condition example. As long as it does not deviate from the main purpose of the present invention and achieves the purpose of the present invention, the present invention can adopt various conditions.
[0131] As a grinding brush, D-100 manufactured by HOTANI Co., Ltd. was used. During grinding, an aqueous solution of 1.0 to 5.0% NaOH was applied to the surface of the steel plate, and grinding was performed under the conditions shown in Table 1. It should be noted that AA in the column of strain treatment conditions in Table 1 means that the brush pressure reduction is 10 mm, A means that the brush pressure reduction is 0.5 mm, and B means that the brush pressure reduction is 0.4 mm. Grinding was performed at a rotation speed of 100 to 1000 rpm.
[0132] Various hot-dip plated steel materials were manufactured by immersing the pre-plated Ni steel materials with strain in various hot-dip plating baths after annealing and scooping them up, thereby attaching a hot-dip plating layer to the surface of the steel materials, and then cooling them by spray cooling until the hot-dip plating layer reaches 300°C just after being scooped up from the hot-dip plating bath. The spraying amount of the spray was set to 0.7 to 32 [L / (mm 2 · minutes)], and the spray time was set to 5 seconds.
[0133] The pre-Ni plated steel material used was a steel material with a Ni plated layer formed on the steel surface. The Ni plated layer adhesion amount was set to 0.8 mg / m 2 In addition, the steel material before the Ni plating is formed is subjected to alkali washing in order to remove dirt and oil adhering to the surface of the steel material. At this time, the surface of the steel material is polished with a metal brush to form a large number of scratches, thereby imparting strain to the surface of the steel material.
[0134] Furthermore, the pre-plated Ni steel material after strain is annealed in a reducing atmosphere. Regarding the annealing conditions, the soaking temperature is set to 580-800°C and the soaking time is set to 10 seconds. The annealing atmosphere is set to a reducing atmosphere containing a mixed gas of hydrogen and nitrogen. Then, the steel material just after annealing is immersed in a hot dip bath.
[0135] The chemical composition of the hot-dip coating is shown in Table 1. It should be noted that in Table 1, the remainder is Zn and impurities. The composition of the pre-plated Ni layer is included in the chemical composition of the hot-dip coating described in Table 1. The manufacturing conditions were set as shown in Table 2. In addition, the metal structure of the coating was evaluated, and the results are shown in Table 3. Furthermore, the surface corrosion resistance and chemical corrosion resistance of the hot-dip coated steel were evaluated, and the results are shown in Table 3.
[0136] The chemical composition of the hot-dip coating and the metal structure of the hot-dip coating were evaluated by the above-mentioned means.
[0137] The evaluation of plane corrosion resistance is set as follows. The obtained hot-dip galvanized steel material is cut into 100 mm × 50 mm and provided for the plane corrosion resistance evaluation test. The evaluation of plane corrosion resistance is carried out by the corrosion promotion test specified in JASO-CCT-M609, and after 120 cycles, it is carried out by comparing the corrosion loss. The evaluation criteria are set as follows, and "AA" and "A" are qualified.
[0138] AA: Corrosion loss less than 40g / m 2
[0139] A: Corrosion loss is 40g / m 2 Above and below 60g / m 2
[0140] B: 60g / m 2 above
[0141] The evaluation of the chemical corrosion resistance is set as follows. A 70×150 mm square test piece is cut out from the obtained hot-dip galvanized steel material, and the JASO test (M609-91) is carried out with the four end faces of the test piece open, and the red rust area ratio of the left and right side faces of the end face after 30 cycles is evaluated. The evaluation criteria of the red rust area ratio are shown below. "AA" and "A" are regarded as qualified.
[0142] AA: Red rust area rate is less than 10%
[0143] A: The red rust area ratio is more than 10% and less than 20%
[0144] B: Red rust area rate is more than 20%
[0145] The chemical composition and metal structure of the hot-dip coating layer of Examples 1 to 25 and 39 to 41 of the present invention are appropriately controlled, and both the flat corrosion resistance and the chemical corrosion resistance are excellent. In addition, the coating weight per single surface of the hot-dip coating layer of the Examples is, for example, 20 to 150 g / m 2 range.
[0146] In Comparative Example 26, the Al content of the hot-dip coating layer was insufficient. Therefore, in Comparative Example 26, the plane corrosion resistance was insufficient.
[0147] In Comparative Example 27, the amount of Al in the hot-dip coating layer was excessive. Therefore, in Comparative Example 27, the chemical corrosion resistance was insufficient.
[0148] In Comparative Example 28, the amount of Mg in the hot-dip coating was insufficient. Therefore, in Comparative Example 28, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0149] In Comparative Example 29, the amount of Mg in the hot-dip coating was excessive. Therefore, in Comparative Example 29, the plane corrosion resistance was insufficient.
[0150] In Comparative Example 30, the amount of Si in the hot-dip coating layer was excessive. Therefore, in Comparative Example 30, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0151] In Comparative Example 31, the amount of Ca in the hot-dip coating layer was excessive. Therefore, in Comparative Example 31, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0152] In Comparative Example 32, the amount of Ni in the hot-dip coating layer was excessive. Therefore, in Comparative Example 32, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0153] In Comparative Example 33, spray cooling was not performed, but air cooling using an inert gas was performed. Therefore, in Comparative Example 33, the α phase and the MgZn2 phase were not randomly oriented. Therefore, in Comparative Example 33, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0154] In Comparative Example 34, the steel material was not plated with Ni. Therefore, in Comparative Example 34, the α phase and the MgZn2 phase were not randomly oriented. Therefore, in Comparative Example 34, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0155] In Comparative Example 35, the spray amount of the spray during spray cooling was less than 1.0 [L / (mm 2 · minutes)]. Therefore, in Comparative Example 35, the α phase and the MgZn2 phase are not randomly oriented. Therefore, in Comparative Example 33, both the plane corrosion resistance and the chemical corrosion resistance are insufficient.
[0156] In Comparative Example 36, the spray volume during spray cooling exceeded 30 [L / (mm 2 · minutes)]. Therefore, the plating appearance became poor in Comparative Example 36. Therefore, in Comparative Example 36, the evaluation of the structure of the plating layer and the evaluation of the flat corrosion resistance and the chemical corrosion resistance could not be carried out.
[0157] In Comparative Examples 37, 38, and 42, the soaking temperature during annealing was 600° C. or higher. Therefore, in Comparative Examples 37, 38, and 42, Ni and Fe were alloyed, the function as the nucleation site of the Ni plating layer disappeared, and the α phase and the MgZn2 phase were not randomly oriented. Therefore, in Comparative Examples 37, 38, and 42, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0158] In Comparative Example 43, since the reduction during grinding was small, strain could not be sufficiently applied. Therefore, the α phase and the MgZn2 phase were not randomly oriented. Therefore, in Comparative Example 43, both the plane corrosion resistance and the chemical corrosion resistance were insufficient.
[0159] [Table 1]
[0160]
[0161] [Table 2]
[0162]
[0163] [Table 3]
[0164]
[0165] Industrial Applicability
[0166] According to the above aspect of the present invention, since both the plane corrosion resistance and the chemical corrosion resistance are excellent, the industrial applicability is high.
Claims
1. A hot-dip galvanized steel material comprising: steel; and A hot-dip coating is disposed on the surface of the steel material. The chemical composition of the hot-dip coating contains, in mass %, the following: Al:10.0~30.0%、 Mg: 4.0-15.0%, Fe: 0.01~15.0%, Si: 0-10.0%, Ni: 0-1.0%, Ca: 0-4.0%, further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less, The rest: contains Zn and impurities, The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2a): 0.5≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2 }≤2.5(1a) 0.2≤I(111) α / I(200) α ≤5.0(2a) in, I(100) in formula (1a) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
2. The hot-dip galvanized steel material according to claim 1, wherein: The Mg content in the chemical composition of the hot-dip coating layer is set to Mg: 5.0 to 15.0% by mass%.
3. The hot-dip galvanized steel material according to claim 1, wherein: The Mg content in the chemical composition of the hot-dip coating layer is set to Mg: 6.0 to 15.0% by mass%.
4. A hot-dip galvanized steel material comprising: steel; and A hot-dip coating is disposed on the surface of the steel material. The chemical composition of the hot-dip coating contains, in mass %, the following: Al:12.0~30.0%、 Mg: 3.0-15.0%, Fe: 0.01~15.0%, Si: 0-10.0%, Ni: 0-1.0%, Ca: 0-4.0%, further containing one or more elements selected from the group consisting of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, and W: 0 to 0.5%, and the total amount of these elements is set to 5% or less, The rest: contains Zn and impurities, The diffraction intensity of the hot-dip galvanized layer obtained from the X-ray diffraction measurement results satisfies the relationship between the following formulas (1a) and (2a): 0.5≤I(100) MgZn2 / {I(002) MgZn2 +I(101) MgZn2 }≤2.5(1a) 0.2≤I(111) α / I(200) α ≤5.0(2a) in, I(100) in formula (1a) MgZn2 is the diffraction intensity of the (100) phase of MgZn2, I(002) MgZn2 is the diffraction intensity of (002) of MgZn2 phase, I(101) MgZn2 is the diffraction intensity of (101) of the MgZn2 phase, I(111) in formula (2a) α is the diffraction intensity of the α phase (111), I(200) α is the diffraction intensity of (200) of the α phase.
5. The hot-dip galvanized steel material according to claim 4, wherein: The Al content in the chemical composition of the hot-dip coating layer is set to be Al: 15.0 to 30.0% by mass%.