Thermal spraying zinc-aluminum alloy wire and preparation method thereof

By adjusting the ratios of Si, Ce, Sc and V in the zinc-aluminum alloy wire to form a dense film layer, the problem of insufficient corrosion resistance and adhesion of thermally sprayed zinc-aluminum alloy wire in the marine environment is solved, and higher resistance is achieved Corrosiveness and adhesion protect the long-term stability of the metal structure.

CN118996314APending Publication Date: 2024-11-22XINXING HEBEI METALLURGY RESOURCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411279435.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing thermally sprayed zinc-aluminum alloy wires are insufficient in corrosion resistance and adhesion in marine environments, making it difficult to protect metal structures for a long time.

Method used

By adjusting the composition of zinc-aluminum alloy wire, especially the ratio of Si, Ce, Sc and V, a dense film layer is formed to improve its corrosion resistance and adhesion. The preparation method includes smelting, refining, annealing and drawing to ensure specific The content and proportion of elements.

Benefits of technology

The corrosion resistance and adhesion of thermally sprayed zinc-aluminum alloy wire is significantly improved, and it can more effectively prevent the intrusion of corrosive media and improve the stability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of thermal spraying alloys, and provides a thermal spraying zinc-aluminum alloy wire and a preparation method thereof.The thermal spraying zinc-aluminum alloy wire is composed of, by weight, 15%-25% of Al, 0.05%-0.6% of Mg, 0.1%-0.5% of Ti, 0.3%-0.8% of Si, 0.05%-0.2% of Ce, 0.005%-0.01% of Sc, 0.03%-0.09% of V and the balance Zn and inevitable impurities. By means of the technical scheme, the problems that in the related technology, thermal spraying zinc-aluminum alloy wires are poor in corrosion resistance and adhesiveness are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal spraying alloys, and in particular to a thermal spraying zinc-aluminum alloy wire and a preparation method thereof. Background Art

[0002] In many industrial fields, the corrosion problem of metal structures has always been a major challenge. Since metal materials are prone to chemical reactions in various environmental conditions, such as the atmosphere, seawater, and soil, the damage to the structure and the decline in performance will shorten the service life of the metal structure and increase maintenance costs and safety risks. In order to protect metal structures from corrosion, people have been seeking effective anti-corrosion methods. As an important surface protection technology, thermal spraying technology plays an increasingly important role in the field of anti-corrosion.

[0003] For a long time, pure zinc thermal spray coatings have been widely used in the corrosion protection of metal structures, but the corrosion resistance of pure zinc coatings also has certain limitations. In some harsh corrosive environments, the life of pure zinc coatings is relatively short. Pure aluminum thermal spray coatings have good oxidation resistance and can form a dense oxide film in the atmosphere to protect the base metal, but the hardness of pure aluminum coatings is low and the wear resistance is poor. In order to overcome the limitations of pure zinc and pure aluminum coatings, people began to study and apply zinc-aluminum alloy thermal spray coatings. The synergistic effect of zinc and aluminum in zinc-aluminum alloys improves the hardness and wear resistance of zinc-aluminum alloy coatings. However, in the marine environment, although zinc-aluminum alloys have certain corrosion resistance, they are still faced with corrosion challenges when exposed to seawater, sea fog and other conditions for a long time. Therefore, the preparation of a corrosion-resistant thermal spray zinc-aluminum alloy wire is a problem that needs to be solved at present. Summary of the invention

[0004] The invention provides a thermal sprayed zinc-aluminum alloy wire and a preparation method thereof, which solves the problems of poor corrosion resistance and poor adhesion of the thermal sprayed zinc-aluminum alloy wire in the related art.

[0005] The technical solution of the present invention is as follows: The invention provides a thermal sprayed zinc-aluminum alloy wire, which consists of the following components by weight percentage: Al 15%-25%, Mg 0.05%-0.6%, Ti 0.1%-0.5%, Si 0.3%-0.8%, Ce 0.05%-0.2%, Sc 0.005%-0.01%, V 0.03%-0.09%, and the balance is Zn and inevitable impurities.

[0006] As a further technical solution, the sum of the weight percentages of Si and Ce is 0.4%≤Si+Ce≤0.85%.

[0007] In the present invention, by limiting 0.4%≤Si+Ce≤0.85%, the zinc-aluminum alloy wire can form a denser film layer during thermal spraying, thereby further improving the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire.

[0008] As a further technical solution, the sum of the weight percentages of Sc and V is 0.04%≤Sc+V≤0.095%.

[0009] In the present invention, by further limiting the sum of the weight percentages of Sc and V to 0.04%≤Sc+V≤0.095% when the sum of the weight percentages of Si and Ce is 0.4%≤Si+Ce≤0.85%, the stability of the thermally sprayed zinc-aluminum alloy wire can be improved, and the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire are further improved.

[0010] As a further technical solution, the ratio of the Sc+V to the Si+Ce is: 0.12≤(Sc+V) / (Si+Ce)≤0.18.

[0011] In the present invention, when the sum of the weight percentages of Si and Ce is 0.4%≤Si+Ce≤0.85% and the sum of the weight percentages of Sc and V is 0.04%≤Sc+V≤0.095%, the ratio of Sc+V to Si+Ce is further limited to: 0.12≤(Sc+V) / (Si+Ce)≤0.18, thereby further improving the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire.

[0012] The present invention also provides a method for preparing a thermally sprayed zinc-aluminum alloy wire, comprising the following steps: S1, mixing the ingredients according to the above, and obtaining a wire blank through smelting, refining and continuous casting; S2. The wire blank is annealed and drawn to obtain a thermally sprayed zinc-aluminum alloy wire.

[0013] As a further technical solution, the smelting temperature is 650-700°C.

[0014] As a further technical solution, the refining temperature is 700-750° C., and the refining time is 1-2 hours.

[0015] As a further technical solution, the annealing temperature is 250-350° C. and the time is 1-2 hours.

[0016] As a further technical solution, the pulling speed is 10 cm / s to 15 cm / s.

[0017] As a further technical solution, the diameter of the thermally sprayed zinc-aluminum alloy wire is 3 mm.

[0018] The working principle and beneficial effects of the present invention are: In the present invention, the thermally sprayed zinc-aluminum alloy wire contains elements such as aluminum, magnesium, titanium, silicon, cerium, ruthenium and platinum in specific proportions, wherein the presence of aluminum helps to form a dense aluminum oxide protective film on the alloy surface to prevent the invasion of corrosive media; and by adding silicon, cerium, ruthenium, platinum and other elements for coordination, the corrosion resistance and adhesion of the zinc-aluminum alloy are further improved, thereby solving the problem of poor corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the following embodiments and comparative examples: Scandium-zinc alloy, scandium content 2wt%; zinc-cerium alloy, cerium content 10wt%; zinc-silicon alloy, silicon content 8wt%; aluminum-vanadium alloy, vanadium content 10wt%; aluminum-titanium alloy, titanium content 5wt%.

[0021] Example 1 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.3%, Ce 0.05%, Sc 0.01%, V 0.09%, the balance is Zn and inevitable impurities; wherein Si+Ce=0.035%, Sc+V=0.1%, (Sc+V) / (Si+Ce)=2.86; The preparation method thereof comprises the following steps: S1. Aluminum ingots, magnesium ingots, scandium-zinc alloy (scandium content 2wt%), zinc-cerium alloy (cerium content 10wt%), zinc-silicon alloy (silicon content 8wt%), aluminum-vanadium alloy (vanadium content 10wt%), aluminum-titanium alloy (titanium content 5wt%), and zinc blocks are mixed according to target composition, smelted at 650° C., refined at 700° C. for 2 h, and then continuously cast to obtain wire blanks; S2. Anneal the wire blank at 250° C. for 2 h, and draw it at a speed of 10 cm / s to obtain a thermally sprayed zinc-aluminum alloy wire with a diameter of 3 mm.

[0022] Example 2 The thermal sprayed zinc-aluminum alloy wire is composed of the following components by weight percentage: Al 20%, Mg 0.35%, Ti 0.25%, Si 0.75%, Ce 0.15%, Sc 0.006%, V 0.031%, and the balance is Zn; wherein Si+Ce=0.9%, Sc+V=0.037%, (Sc+V) / (Si+Ce)=0.04; The preparation method thereof comprises the following steps: S1. Aluminum ingots, magnesium ingots, scandium-zinc alloy (scandium content 2wt%), zinc-cerium alloy (cerium content 10wt%), zinc-silicon alloy (silicon content 8wt%), aluminum-vanadium alloy (vanadium content 10wt%), aluminum-titanium alloy (titanium content 5wt%), and zinc blocks are mixed according to target composition, smelted at 680° C., refined at 720° C. for 2 h, and then continuously cast to obtain wire blanks; S2. Anneal the wire blank at 300° C. for 1 h, and draw it at a speed of 12 cm / s to obtain a thermally sprayed zinc-aluminum alloy wire with a diameter of 3 mm.

[0023] Example 3 The thermal sprayed zinc-aluminum alloy wire is composed of the following components by weight percentage: Al 25%, Mg 0.6%, Ti 0.5%, Si 0.8%, Ce 0.2%, Sc 0.005%, V 0.03%, and the balance is Zn; wherein Si+Ce=1%, Sc+V=0.035%, (Sc+V) / (Si+Ce)=0.035; The preparation method thereof comprises the following steps: S1. Aluminum ingots, magnesium ingots, scandium-zinc alloy (scandium content 2wt%), zinc-cerium alloy (cerium content 10wt%), zinc-silicon alloy (silicon content 8wt%), aluminum-vanadium alloy (vanadium content 10wt%), aluminum-titanium alloy (titanium content 5wt%), and zinc blocks are mixed according to target composition, smelted at 700° C., refined at 750° C. for 1 h, and then continuously cast to obtain wire blanks; S2. The wire blank is annealed at 350° C. for 1 h, and drawn at a speed of 15 cm / s to obtain a thermally sprayed zinc-aluminum alloy wire with a diameter of 3 mm.

[0024] Example 4 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.8%, Ce 0.2%, Sc 0.01%, V 0.09%, and the balance is Zn; wherein Si+Ce=1%, Sc+V=0.1%, (Sc+V) / (Si+Ce)=0.1; The preparation method is the same as that of Example 1.

[0025] Example 5 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.32%, Ce 0.08%, Sc 0.01%, V 0.09%, and the balance is Zn; wherein Si+Ce=0.4%, Sc+V=0.1%, (Sc+V) / (Si+Ce)=0.25; The preparation method is the same as that of Example 1.

[0026] Example 6 The thermal sprayed zinc-aluminum alloy wire is composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.01%, V 0.09%, and the balance is Zn; wherein Si+Ce=0.5%, Sc+V=0.1%, (Sc+V) / (Si+Ce)=0.2; The preparation method is the same as that of Example 1.

[0027] Example 7 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.7%, Ce 0.15%, Sc 0.01%, V 0.09%, and the balance is Zn; wherein Si+Ce=0.85%, Sc+V=0.1%, (Sc+V) / (Si+Ce)=0.118; The preparation method is the same as that of Example 1.

[0028] Example 8 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.005%, V 0.03%, and the balance is Zn; wherein Si+Ce=0.5%, Sc+V=0.035%, (Sc+V) / (Si+Ce)=0.07; The preparation method is the same as that of Example 1.

[0029] Example 9 The thermal sprayed zinc-aluminum alloy wire is composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.008%, V 0.032%, and the balance is Zn; wherein Si+Ce=0.5%, Sc+V=0.04%, (Sc+V) / (Si+Ce)=0.08; The preparation method is the same as that of Example 1.

[0030] Example 10 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.005%, V 0.09%, balance Zn; wherein Si+Ce=0.5%, Sc+V=0.095%, (Sc+V) / (Si+Ce)=0.19; A method for preparing a thermally sprayed zinc-aluminum alloy wire is the same as that in Example 1.

[0031] Embodiment 11 The thermal sprayed zinc-aluminum alloy wire is composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.007%, V 0.053%, and the balance is Zn; wherein Si+Ce=0.5%, Sc+V=0.06%, (Sc+V) / (Si+Ce)=0.12; A method for preparing a thermally sprayed zinc-aluminum alloy wire is the same as that in Example 1.

[0032] Example 12 Thermal sprayed zinc-aluminum alloy wire, composed of the following components by weight percentage: Al 15%, Mg 0.05%, Ti 0.1%, Si 0.4%, Ce 0.1%, Sc 0.01%, V 0.08%, balance Zn; wherein Si+Ce=0.5%, Sc+V=0.09%, (Sc+V) / (Si+Ce)=0.18; A method for preparing a thermally sprayed zinc-aluminum alloy wire is the same as that in Example 1.

[0033] Comparative Example 1 The only difference between this comparative example and Example 1 is that the thermally sprayed zinc-aluminum alloy wire does not contain Si.

[0034] Comparative Example 2 The only difference between this comparative example and Example 1 is that the thermally sprayed zinc-aluminum alloy wire does not contain Ce.

[0035] Comparative Example 3 The only difference between this comparative example and Example 1 is that the thermally sprayed zinc-aluminum alloy wire does not contain Sc.

[0036] Comparative Example 4 The only difference between this comparative example and Example 1 is that the thermally sprayed zinc-aluminum alloy wire does not contain V.

[0037] The zinc-aluminum alloy wires prepared in Examples 1 to 12 and Comparative Examples 1 to 4 were respectively thermally sprayed on the surface of a Q345 steel plate to obtain a steel plate with a zinc-aluminum alloy coating. The coating thickness was 60 μm. The corrosion resistance and adhesion properties of the zinc-aluminum alloy coating were tested. The specific test method is as follows: Adhesion: A hydraulic universal testing machine (model: WES-600D-600kN) was used to measure the adhesion (pulling) of the zinc-aluminum alloy coating on the surface of the Q345 steel plate; Corrosion resistance: Carry out a neutral salt spray test according to the test method in GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test" and record the time when red rust appears on the steel plate; The test results are shown in Table 1.

[0038] Table 1 Performance test results of thermal sprayed zinc-aluminum alloy wire

[0039] Compared with Example 1, Comparative Example 1 does not contain Si, Comparative Example 2 does not contain Ce, Comparative Example 3 does not contain Sc, and Comparative Example 4 does not contain V. As a result, the adhesion (drawing) and the time for the appearance of red rust of the thermally sprayed zinc-aluminum alloy wires prepared in Comparative Examples 1 to 4 are lower than those in Example 1, indicating that the simultaneous inclusion of Si, Ce, Sc, and V components can improve the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wires.

[0040] Compared with Example 1, the percentage content of Si+Ce was changed in Examples 4 to 7. As a result, the adhesion (drawing) and the time for the appearance of red rust of the thermally sprayed zinc-aluminum alloy wires prepared in Examples 5 to 7 were higher than those in Examples 1 and 4, indicating that when 0.4%≤Si+Ce≤0.85%, the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wires can be further improved.

[0041] Compared with Example 6, the percentage content of Sc+V was changed in Examples 8 to 10. As a result, the adhesion (drawing) and the time for the appearance of red rust of the thermally sprayed zinc-aluminum alloy wire prepared in Examples 9 to 10 were higher than those in Examples 6 and 8, indicating that when 0.04%≤Sc+V≤0.095%, the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire can be further improved.

[0042] Compared with Example 10, the ratio of Sc+V to Si+Ce was changed in Examples 11-12. As a result, the adhesion (pulling) and the time for the appearance of red rust of the sprayed zinc-aluminum alloy wire prepared in Examples 11-12 were higher than those in Example 10, indicating that when 0.12≤(Sc+V) / (Si+Ce)≤0.18, the corrosion resistance and adhesion of the thermally sprayed zinc-aluminum alloy wire can be further improved.

[0043] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A thermal sprayed zinc-aluminum alloy wire, It is characterized in that Calculated by weight percentage, it is composed of the following components: Al 15%~25%, Mg 0.05%~0.6%, Ti 0.1%~0.5%, Si 0.3%~0.8%, Ce 0.05%~0.2%, Sc 0.005%~0.01%, V0.03%~0.09%, and the balance is Zn and inevitable impurities.

2. A thermally sprayed zinc-aluminum alloy wire according to claim 1, It is characterized in that The sum of the weight percentages of Si and Ce is 0.4%≤Si+Ce≤0.85%.

3. A thermally sprayed zinc-aluminum alloy wire according to claim 2, It is characterized in that The sum of the weight percentages of Sc and V is 0.04%≤Sc+V≤0.095%.

4. A thermally sprayed zinc-aluminum alloy wire according to claim 3, It is characterized in that The ratio of the Sc+V to the Si+Ce is: 0.12≤(Sc+V) / (Si+Ce)≤0.

18.

5. A method for preparing a thermally sprayed zinc-aluminum alloy wire according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1, mixing the ingredients according to the above, and obtaining a wire blank through smelting, refining and continuous casting; S2. The wire blank is annealed and drawn to obtain a thermally sprayed zinc-aluminum alloy wire.

6. A method for preparing a thermally sprayed zinc-aluminum alloy wire according to claim 5, It is characterized in that The smelting temperature is 650-700°C.

7. A method for preparing a thermally sprayed zinc-aluminum alloy wire according to claim 5, It is characterized in that The refining temperature is 700-750° C., and the refining time is 1-2 hours.

8. A method for preparing a thermally sprayed zinc-aluminum alloy wire according to claim 5, It is characterized in that The annealing temperature is 250-350° C. and the annealing time is 1-2 hours.

9. A method for preparing a thermally sprayed zinc-aluminum alloy wire according to claim 5, It is characterized in that The pulling speed is 10 cm / s to 15 cm / s.