Carbon anode plate for electrolytic fluorine preparation and preparation method thereof
By immersing a metal salt thermosetting impregnant on the carbon anode plate and calcining it to form metal oxides, the problems of increasing resistance and anode polarization of the carbon anode plate during electrolytic fluorine production are solved, which extends the use time and reduces production costs.
Patent Information
- Application Number
- CN202411009846.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
AI Technical Summary
During the electrolytic fluorine-making process, the carbon anode plate has an increase in resistance due to the formation of C-F polymer layer on the surface, which is prone to anode polarization and fracture, reducing usage time and increasing production costs.
By immersing a thermosetting impregnant containing metal salt into the pores and surface of the carbon anode plate and calcining under vacuum, the metal salt is carbonized to form an electrolytic fluorine-making carbon anode plate containing metal oxides, thereby improving its conductivity and Compressive strength blocks the anode effect.
It effectively extends the use time of carbon anode plate, reduces production costs, improves the kinetics and conductivity of fluorine precipitation reaction, and reduces the generation of impurity gases.
Smart Images

Figure CN118996466A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon anode plates, and in particular to a carbon anode plate for electrolytic fluorine production and a preparation method thereof. Background Art
[0002] Fluorine gas is active and highly oxidizing. It can react with most inorganic or organic substances at room temperature or below and release a large amount of heat. It is an efficient fluorinating agent for preparing a variety of fluorides and has been widely used in the fields of chemical industry, medicine, daily chemicals, nuclear industry, etc. So far, electrolytic fluorine production is the only method that can produce fluorine gas on a large scale industrially, and the anode plate is an extremely critical material in the fluorine gas production process, which has an important impact on the efficiency of electrolytic fluorine production.
[0003] Carbon plates are widely used in the electrolytic fluorine industry as a common anode material. However, when the electrolytic cell is running for a long time, a CF polymer layer is formed on the surface of the carbon anode, causing the resistance to increase, and it is easy to produce anode polarization, carbon anode breakage and other phenomena, and produce a large amount of impurity gas, which reduces the service life of the carbon anode, prolongs the production cycle, and increases the production cost. Summary of the invention
[0004] Based on this, the present invention proposes a carbon anode plate for electrolytic fluorine production and a preparation method thereof. The modified carbon anode plate not only has reduced porosity and increased strength, but can also form graphite embedded compounds during the process of electrolytic fluorine production to improve conductivity, while the surface remains flat, effectively blocking the anode effect.
[0005] According to a first aspect of the present invention, there is provided a method for preparing a carbon anode plate for electrolytic fluorine production, comprising:
[0006] By impregnating a thermosetting impregnant containing a metal salt into the pores and surface of the carbon anode plate;
[0007] The metal salt and the thermosetting impregnating agent in the pores and on the surface of the carbon anode plate are carbonized by calcination to form a carbon anode plate for electrolytic fluorine production containing metal oxides.
[0008] According to an embodiment of the present invention, the following steps are included:
[0009] Under vacuum conditions, the carbon anode plate is impregnated with the thermosetting impregnant containing the metal salt;
[0010] The carbon anode plate after impregnation is taken out and baked in an inert atmosphere to obtain the modified carbon anode plate for electrolytic fluorine production;
[0011] Wherein, the metal salt is one or more of nitrates, sulfates and chlorides of Al, Ni, Cu, Mg, Li and Ag.
[0012] According to an embodiment of the present invention, the step of impregnating the carbon anode plate with a thermosetting impregnant containing a metal salt under vacuum conditions comprises:
[0013] Putting the vacuum-dried carbon anode plate into a reaction kettle and drawing a vacuum;
[0014] A preheated thermosetting impregnating agent containing a metal salt is added into the reaction kettle to impregnate the carbon anode plate.
[0015] According to an embodiment of the present invention, after the vacuum is extracted, the pressure in the reactor is less than 0.1 MPa.
[0016] According to an embodiment of the present invention, the thermosetting impregnating agent includes one or both of a thermosetting unsaturated resin and an epoxy resin;
[0017] And / or, the concentration of the metal salt contained in the thermosetting impregnating agent is 1% to 5%.
[0018] According to an embodiment of the present invention, the preheating temperature of the thermosetting impregnating agent is 30°C to 60°C.
[0019] According to an embodiment of the present invention, the immersion temperature of the carbon anode plate is 30° C. to 60° C., the immersion time is 0.5 h to 3 h, and the immersion pressure is 0.1 MPa to 0.5 MPa.
[0020] According to an embodiment of the present invention, the inert atmosphere for baking the carbon anode plate is nitrogen or argon.
[0021] According to an embodiment of the present invention, the carbon anode plate after impregnation is taken out and baked in an inert atmosphere to obtain the modified carbon anode plate for electrolytic fluorine production, comprising:
[0022] The impregnated carbon anode plate is subjected to a first-stage calcination at 200° C. to 340° C.;
[0023] The carbon anode plate which has been calcined in the first stage is calcined in the second stage at 450° C. to 550° C.;
[0024] The carbon anode plate that has been calcined in the second stage is calcined in the third stage at 900° C. to 1100° C. to obtain the modified carbon anode plate for electrolytic fluorine production.
[0025] According to an embodiment of the present invention, the holding time of the first stage calcination, the second stage calcination and the third stage calcination is 1 hour, and the heating rate is 2°C / min to 10°C / min.
[0026] According to a second aspect of the present invention, there is provided a carbon anode plate for electrolytic fluorine production obtained by the above-mentioned preparation method, wherein the carbon anode plate for electrolytic fluorine production contains metal oxides and carbonized thermosetting impregnating agent in the pores and on the surface.
[0027] It can be seen from the above technical scheme that the method for preparing a carbon anode plate for electrolytic fluorine production provided by the present invention has the following beneficial effects:
[0028] (1) The present invention first dries the carbon anode plate and then impregnates it with metal nitrate or sulfate and unsaturated resin to embed the carbon anode plate so that the F on the surface of the carbon anode forms a nearly ionic bond with graphite during electrolysis, and the surface remains flat after treatment. This structure can effectively block the anode effect of the carbon anode plate when the electrolytic cell is working.
[0029] (2) The present invention adds metal salts to the impregnation solution of the carbon anode plate, which can not only improve the compressive strength of the carbon anode plate itself, but also the metal fluoride generated during the electrolysis process can improve the wettability of the electrode surface, making fluoride ions easier to adsorb and the generated gas easier to desorb.
[0030] (3) The present invention also improves the kinetics of the fluorine precipitation reaction and the conductivity of the carbon anode plate by modifying the surface of the carbon anode plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The influence of the immersion time on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention;
[0032] Figure 2 The influence of the immersion pressure on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention;
[0033] Figure 3 The influence of the immersion temperature on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention;
[0034] Figure 4 The effects of adding different solid transition metal salts on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 13 and Examples 15-19 of the present invention;
[0035] Figure 5 The effects of adding different concentrations of metal salts on key indicators of carbon anode plates for electrolytic fluorine production in Examples 1-5 of the present invention;
[0036] Figure 6 The effects of different calcination methods on the key indicators of carbon anode plates in Example 20 of the present invention and Comparative Example 1;
[0037] Figure 7This is the effect of different modification methods of Example 1 of the present invention and Comparative Example 2 on the key indicators of the carbon anode plate. DETAILED DESCRIPTION
[0038] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0039] Carbon plates are widely used in the electrolytic fluorine industry as a common anode material. However, when the electrolytic cell is running for a long time, a CF polymer layer is formed on the surface of the carbon anode, causing the resistance to increase, and it is easy to produce anode polarization, carbon anode fracture and other phenomena, and produce a large amount of impurity gas, which reduces the service life of the carbon anode, prolongs the production cycle, and increases the production cost. Therefore, a new preparation method of carbon anode plates for electrolytic fluorine is needed, so that the prepared carbon anode plates for electrolytic fluorine can alleviate the problem of CF polymer layer formed on the surface of the carbon anode after long-term operation, thereby reducing the resistance increase, easy to produce anode polarization, carbon anode fracture, and produce a large amount of impurity gas and other phenomena, further prolonging the service life of the carbon anode, shortening the production cycle, and reducing production costs.
[0040] According to a first aspect of the present invention, there is provided a method for preparing a carbon anode plate for electrolytic fluorine production, comprising:
[0041] By impregnating a thermosetting impregnant containing a metal salt into the pores and surface of the carbon anode plate;
[0042] The metal salt and the thermosetting impregnant in the pores and on the surface of the carbon anode plate are carbonized by calcination to form a carbon anode plate for electrolytic fluorine production containing metal oxides.
[0043] The present invention first dries the carbon anode plate and then impregnates it with metal nitrate or sulfate and unsaturated resin to embed the carbon anode plate so that F on the surface of the carbon anode forms a nearly ionic bond with graphite during electrolysis, and the surface remains flat after treatment, which can effectively block the anode effect of the carbon anode plate when the electrolytic cell is working.
[0044] The invention adds metal salts to the impregnation solution of the carbon anode plate, which can not only improve the compressive strength of the carbon anode plate itself, but also the metal fluoride generated during the electrolysis process can improve the wettability of the electrode surface, making fluoride ions easier to adsorb and the generated gas easier to desorb.
[0045] According to an embodiment of the present invention, the following steps are included:
[0046] Under vacuum conditions, the carbon anode plate is impregnated with a thermosetting impregnant containing a metal salt;
[0047] The impregnated carbon anode plate is taken out and baked in an inert atmosphere to obtain a modified carbon anode plate for electrolytic fluorine production;
[0048] The metal salt is one or more of nitrates, sulfates and chlorides of Al, Ni, Cu, Mg, Li and Ag.
[0049] According to an embodiment of the present invention, the carbon anode plate is impregnated with a thermosetting impregnant containing a metal salt under vacuum conditions, including:
[0050] Put the vacuum-dried carbon anode plate into a reaction kettle and draw a vacuum;
[0051] A preheated thermosetting impregnant containing a metal salt is added into a reaction kettle to impregnate the carbon anode plate.
[0052] According to an embodiment of the present invention, after the vacuum is drawn, the pressure in the reactor is less than 0.1 MPa.
[0053] According to an embodiment of the present invention, the thermosetting impregnating agent includes one or both of a thermosetting unsaturated resin and an epoxy resin;
[0054] And / or, the concentration of the metal salt contained in the thermosetting impregnating agent is 1% to 5%.
[0055] According to an embodiment of the present invention, the preheating temperature of the thermosetting impregnating agent is 30°C to 60°C.
[0056] According to an embodiment of the present invention, the immersion temperature of the carbon anode plate is 30° C. to 60° C., the immersion time is 0.5 h to 3 h, and the immersion pressure is 0.1 MPa to 0.5 MPa.
[0057] According to an embodiment of the present invention, the inert atmosphere for baking the carbon anode plate is nitrogen or argon.
[0058] According to an embodiment of the present invention, the impregnated carbon anode plate is taken out and baked in an inert atmosphere to obtain a modified carbon anode plate for electrolytic fluorine production, comprising:
[0059] The impregnated carbon anode plate is subjected to first-stage calcination at 200°C to 340°C;
[0060] The carbon anode plate which has been calcined in the first stage is calcined in the second stage at 450° C. to 550° C.;
[0061] The carbon anode plate which has been calcined in the second stage is calcined in the third stage at 900° C. to 1100° C. to obtain a modified carbon anode plate for electrolytic fluorine production.
[0062] According to an embodiment of the present invention, the holding time of the first stage calcination, the second stage calcination and the third stage calcination is 1 hour, and the heating rate is 2° C. / min to 10° C. / min.
[0063] According to a second aspect of the present invention, there is provided a carbon anode plate for electrolytic fluorine production obtained by the above-mentioned preparation method, wherein the carbon anode plate for electrolytic fluorine production contains metal oxides and carbonized thermosetting impregnating agent in the pores and on the surface.
[0064] The present invention embeds the carbon anode plate so that the F on the surface of the carbon anode forms a nearly ionic bond with graphite during electrolysis, and the surface remains flat after treatment. It can effectively block the anode effect of the carbon anode plate when the electrolytic cell is working, and the surface modification of the carbon anode plate improves the kinetics of the fluorine precipitation reaction and the conductivity of the carbon anode plate.
[0065] The technical solution of the present invention is described in detail below through preferred embodiments. It should be noted that the specific embodiments below are only used for illustration and are not used to limit the present invention.
[0066] Example 1
[0067] The vacuum-dried carbon anode plate was placed in a reactor and vacuum was drawn to a vacuum degree of 0.1 MPa and maintained for 5 min. Subsequently, an unsaturated resin containing 1% Al(NO3)3 was preheated at 60°C and slowly added to the reactor. The carbon anode plate was immersed at a constant 30°C and 0.3 MPa for 2 h.
[0068] After the impregnation is completed, the carbon anode plate is taken out, and after pre-curing, it is baked in a nitrogen atmosphere using a temperature increase curve of 5°C / min, staying at 270°C for 1 hour, staying at 500°C for 1 hour, and finally staying at 1000°C for 2 hours to obtain a modified carbon anode plate for electrolytic fluorine production.
[0069] Example 2
[0070] The specific steps are the same as those of Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 2% Al(NO3)3.
[0071] Example 3
[0072] The specific steps are the same as those of Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 3% Al(NO3)3.
[0073] Example 4
[0074] The specific steps are the same as those in Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 4% Al(NO3)3.
[0075] Example 5
[0076] The specific steps are the same as those of Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 5% Al(NO3)3.
[0077] Example 6
[0078] The specific steps are the same as those in Example 1, except that the immersion time of the carbon anode plate is 1 hour.
[0079] Example 7
[0080] The specific steps are the same as those in Example 1, except that the immersion time of the carbon anode plate is 0.5 h.
[0081] Example 8
[0082] The specific steps are the same as those in Example 1, except that the immersion time of the carbon anode plate is 3 hours.
[0083] Example 9
[0084] The specific steps are the same as those in Example 1, except that the immersion temperature of the carbon anode plate is 40°C.
[0085] Example 10
[0086] The specific steps are the same as those in Example 1, except that the immersion temperature of the carbon anode plate is 50°C.
[0087] Embodiment 11
[0088] The specific steps are the same as those in Example 1, except that the immersion temperature of the carbon anode plate is 60°C.
[0089] Example 12
[0090] The specific steps are the same as those in Example 10, except that the immersion pressure of the carbon anode plate is 0.5 MPa.
[0091] Embodiment 13
[0092] The specific steps are the same as those in Example 10, except that the immersion pressure of the carbon anode plate is 0 MPa.
[0093] Embodiment 14
[0094] The specific steps are the same as those in Example 10, except that the immersion pressure of the carbon anode plate is 0.1 MPa.
[0095] Embodiment 15
[0096] The specific steps are the same as those in Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 1% Ni(NO3)3.
[0097] Example 16
[0098] The specific steps are the same as those in Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 1% Cu(NO3)3.
[0099] Embodiment 17
[0100] The specific steps are the same as those in Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 1% Mg(NO3)3.
[0101] Embodiment 18
[0102] The specific steps are the same as those in Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 1% Li(NO3)3.
[0103] Embodiment 19
[0104] The specific steps are the same as those of Example 1, except that the thermosetting impregnating agent containing a metal salt is an unsaturated resin containing 1% Ag(NO3)3.
[0105] Embodiment 20
[0106] The specific steps are the same as those in Example 15, except that after pre-curing, the plate is calcined in a nitrogen atmosphere at a temperature rise rate of 5°C / min, staying at 200°C for 1 hour, staying at 500°C for 1 hour, and finally staying at 1000°C for 2 hours to obtain a modified carbon anode plate for electrolytic fluorine production.
[0107] Comparative Example 1:
[0108] The specific steps are the same as those in Example 15, except that after pre-curing, the temperature is increased from 200°C to 1000°C at a rate of 5°C / min in a nitrogen atmosphere and kept there for 4 hours to obtain a carbon anode plate.
[0109] Comparative Example 2:
[0110] The carbon anode plate is modified by depositing metal Al salt on the surface of the carbon anode plate.
[0111] Experimental Example 1:
[0112] Figure 1 It is the influence of the immersion time on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention.
[0113] Figure 1 (a) is the effect of immersion time on the weight gain rate of carbon anode plates for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention.
[0114] Figure 1 (b) is the effect of immersion time on the porosity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention.
[0115] Figure 1(c) is the effect of immersion time on the strength of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention.
[0116] Figure 1 (d) is the effect of immersion time on the resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 of the present invention.
[0117] The effect of immersion time on the weight gain, porosity, strength and resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 6-8 was investigated. Figure 1 As shown in the figure, when the immersion time is 0.5-3h, the immersion time has little effect on the resistivity, but when the immersion time is 0.5h, the immersion degree of the carbon anode plate for electrolytic fluorine production is incomplete, so the weight gain rate, strength and porosity are poor. After the immersion time is 1h, the immersion degree is high, so the immersion time after 1h has little effect on the weight gain rate, strength and porosity of the carbon anode plate for electrolytic fluorine production.
[0118] Experimental Example 2:
[0119] Figure 2 It is the influence of the immersion pressure on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention.
[0120] Figure 2 (a) is the effect of immersion pressure on the weight gain rate of carbon anode plates for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention.
[0121] Figure 2 (b) is the effect of the immersion pressure on the porosity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention.
[0122] Figure 2 (c) is the effect of immersion pressure on the strength of carbon anode plates for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention.
[0123] Figure 2 (d) is the effect of the immersion pressure on the resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 12-13 of the present invention.
[0124] The effect of the immersion pressure on the weight gain, porosity, strength and resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 12-13 was investigated. Figure 2 As shown in Figure 2, when the impregnation pressure is between 0 and 0.5 MPa, the impregnation pressure has little effect on the porosity and resistivity, but has a certain effect on the strength and weight gain rate. Figure 2It can be seen that when the immersion pressure is low, the weight gain rate and strength of the carbon anode plate for electrolytic fluorine production are relatively poor. When the immersion pressure reaches 0.1MPa, the weight gain rate of the carbon anode plate for electrolytic fluorine production reaches a stable level. When the immersion pressure reaches 0.3MPa, the strength of the carbon anode plate for electrolytic fluorine production reaches a stable level. When the immersion pressure reaches 0.3MPa, the strength of the carbon anode plate for electrolytic fluorine production is the best.
[0125] Experimental Example 3:
[0126] Figure 3 It is the influence of the immersion temperature on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention.
[0127] Figure 3 (a) is the effect of immersion temperature on the strength improvement rate of carbon anode plates for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention.
[0128] Figure 3 (b) is the effect of the immersion temperature on the strength improvement rate of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention.
[0129] Figure 3 (c) is the effect of the immersion temperature on the porosity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention.
[0130] Figure 3 (d) is the effect of the immersion temperature on the resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 of the present invention.
[0131] The effect of the immersion temperature on the weight gain, porosity, strength and resistivity of the carbon anode plate for electrolytic fluorine production in Example 1 and Examples 9-11 was investigated. Figure 3 As shown, the higher the immersion temperature, the better the immersion effect of the carbon anode plate. When the immersion temperature reaches 50°C, the immersion degree is high. Therefore, when the immersion temperature reaches 50°C, it has little effect on the weight gain rate, strength and porosity of the carbon anode plate for electrolytic fluorine production.
[0132] Experimental Example 4:
[0133] Figure 4 This is the effect of adding different solid transition metal salts on the key indicators of the carbon anode plate for electrolytic fluorine production in Example 13 and Examples 15-19 of the present invention.
[0134] The effects of adding different solid transition metal salts on the porosity and resistivity of the carbon anode plate for electrolytic fluorine production in Example 13 and Examples 15-19 were investigated. Figure 4As shown in the figure, the addition of metal salts significantly reduces the porosity of the carbon anode plate. The main reason is that the metal ions are oxidized during the carbonization process to form oxides of different sizes that block the pores of the carbon anode plate. At the same time, after modification with metal salts, the resistivity of the carbon anode plate also decreases. The main reason is that the addition of metals improves the charge transfer efficiency and reduces the resistivity. Due to the different electron transfer capabilities of different metals, the modified carbon anode plates have different resistivities.
[0135] Experimental Example 5:
[0136] Figure 5 The invention relates to the effects of adding different concentrations of metal salts on the key indicators of carbon anode plates for electrolytic fluorine production in Examples 1-5 of the present invention.
[0137] The effects of adding different concentrations of metal salts on the porosity and resistivity of the carbon anode plate for electrolytic fluorine production in Examples 1-5 were investigated. Figure 5 Adding different metal salt concentrations has a significant effect on its porosity and resistivity. With the increase of metal salt concentration, the porosity tends to increase, while the resistivity tends to decrease first and then increase. The main reason is that too much metal salt agglomerates during the carbonization process, resulting in an increase in resistivity.
[0138] Experimental Example 6:
[0139] Figure 6 This is the effect of different calcining methods on the key indicators of carbon anode plates in Example 20 of the present invention and Comparative Example 1.
[0140] The effects of different calcination methods on the porosity and resistivity of the carbon anode plate in Example 20 and Comparative Example 1 were investigated. Figure 6 As shown. The performance improvement of the carbon anode plate by three-stage calcination is significantly higher than that by one-stage calcination. The main reason is that the impregnant has three main processes in the carbonization process, namely polycondensation, decomposition and carbonization. The three-stage calcination gives each stage sufficient reaction time, which can greatly improve the performance of the anode plate.
[0141] Experimental Example 7:
[0142] Figure 7 This is the effect of different modification methods of Example 1 of the present invention and Comparative Example 2 on the key indicators of the carbon anode plate.
[0143] The effects of different modification methods of Example 1 and Comparative Example 2 on the porosity and resistivity of the carbon anode plate were investigated. Figure 7 The performance of the carbon anode plate prepared by the impregnation method is significantly higher than that of the carbon anode plate prepared by the deposition method. The main reason is that the deposition method mainly modifies the surface of the carbon anode plate, while the impregnation method is that the impregnation liquid repeatedly enters the interior of the carbon anode plate, and after carbonization, it can effectively block the pores of the carbon anode plate, thereby improving the performance of the carbon anode plate.
[0144] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a carbon anode plate for electrolytic fluorine production, characterized in that: include: By impregnating a thermosetting impregnant containing a metal salt into the pores and surface of the carbon anode plate; The metal salt and the thermosetting impregnating agent in the pores and on the surface of the carbon anode plate are carbonized by calcination to form a carbon anode plate for electrolytic fluorine production containing metal oxides.
2. The preparation method according to claim 1, characterized in that: The steps include: Under vacuum conditions, using the thermosetting impregnating agent containing the metal salt to impregnate the carbon anode plate; The carbon anode plate after impregnation is taken out and baked in an inert atmosphere to obtain the modified carbon anode plate for electrolytic fluorine production; Wherein, the metal salt is one or more of nitrates, sulfates and chlorides of Al, Ni, Cu, Mg, Li and Ag.
3. The preparation method according to claim 2, characterized in that: The method of impregnating the carbon anode plate with a thermosetting impregnant containing a metal salt under vacuum conditions comprises: Putting the vacuum-dried carbon anode plate into a reaction kettle and drawing a vacuum; A preheated thermosetting impregnating agent containing a metal salt is added into the reaction kettle to impregnate the carbon anode plate.
4. The preparation method according to claim 3, characterized in that: After the vacuum is drawn, the pressure in the reactor is less than 0.1 MPa.
5. The preparation method according to claim 1, characterized in that: The thermosetting impregnating agent includes one or both of a thermosetting unsaturated resin and an epoxy resin; And / or, the concentration of the metal salt contained in the thermosetting impregnating agent is 1% to 5%.
6. The preparation method according to claim 2, characterized in that: The preheating temperature of the thermosetting impregnating agent is 30°C to 60°C; And / or, the immersion temperature of the carbon anode plate is 30° C. to 60° C., the immersion time is 0.5 h to 3 h, and the immersion pressure is 0.1 MPa to 0.5 MPa.
7. The preparation method according to claim 2, characterized in that: The inert atmosphere for baking the carbon anode plate is nitrogen or argon.
8. The preparation method according to claim 2, characterized in that: The carbon anode plate after impregnation is taken out and baked in an inert atmosphere to obtain the modified carbon anode plate for electrolytic fluorine production, comprising: The impregnated carbon anode plate is subjected to a first-stage calcination at 200° C. to 340° C.; The carbon anode plate which has been calcined in the first stage is calcined in the second stage at 450° C. to 550° C.; The carbon anode plate that has been calcined in the second stage is calcined in the third stage at 900° C. to 1100° C. to obtain the modified carbon anode plate for electrolytic fluorine production.
9. The preparation method according to claim 8, characterized in that: The holding time of the first stage calcination, the second stage calcination and the third stage calcination is 1 hour, and the heating rate is 2°C / min to 10°C / min.
10. A carbon anode plate for electrolytic fluorine production obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The carbon anode plate for electrolytic fluorine production contains metal oxides and carbonized thermosetting impregnating agents in the holes and on the surface.