Multi-element oxide electrode and preparation method thereof

By adding and evaporating the metal salt solution on the metal substrate, vacuum calcining is solved, the ratio of multi-oxide catalyst elements and low raw material utilization is achieved, and efficient multi-oxide electrode preparation is achieved, which improves catalytic activity and industrial application. sex.

CN118996491AInactive Publication Date: 2024-11-22CRINM (GUANGDONG) INST FOR ADVANCED MATERIALS & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411182962.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to accurately regulate the proportion of elements and improve the utilization rate of raw materials when preparing multi-oxide catalysts, resulting in low catalytic activity and the preparation process is not suitable for large-scale industrialization.

Method used

Using ethanol as a solvent, the reducing agent and metal salt are prepared into a mixed solution, added dropwise on the heated metal substrate and evaporated, and then calcined under a vacuum environment to form a multi-oxide electrode, achieving precise regulation of element ratio and high raw material utilization Rate.

Benefits of technology

It improves catalytic activity and raw material utilization, and forms a multi-oxide electrode with strong binding force with metal substrates, which is suitable for large-scale industrial preparation and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996491A_ABST
    Figure CN118996491A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-element oxide electrode and a preparation method thereof, and belongs to the technical field of hydrogen energy material preparation, and the preparation method comprises the following steps: preparing a reducing agent and at least two metal salts into an ethanol mixed solution; the metal substrate is placed in a heating environment, the mixed solution is repeatedly dropwise added to one face of the metal substrate and volatilized until half of the mixed solution is volatilized, and the metal substrate is turned over to continue the same operation; and calcining the metal substrate in a vacuum environment, and naturally cooling to obtain the multi-element oxide electrode. According to the method, the raw materials can be almost bonded on the metal substrate without excess and loss, the utilization rate of the raw materials is extremely high, the universality is wide, the influence of different bonding difficulty degrees of different raw materials and the same substrate can be eliminated, the proportion and content of metal salts attached to the metal substrate can be accurately regulated and controlled, and the method is suitable for industrial production. And a compact multi-element metal oxide electrode can be formed on the metal substrate only through simple calcination subsequently.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multi-element oxide electrode and a preparation method thereof, belonging to the technical field of hydrogen energy material preparation. Background Art

[0002] With the massive consumption of traditional energy, the energy crisis is becoming more and more severe. Therefore, it is urgent to seek suitable renewable energy. Hydrogen energy can be obtained in large quantities by coupling photovoltaic power generation with water electrolysis to produce hydrogen, and is considered to be one of the cleanest energy sources at present.

[0003] During the water electrolysis process, the oxidation process at the anode end involves four-electron transfer, and the reaction rate is lower than that at the cathode end, thus becoming the rate-determining step that restricts the water electrolysis reaction.

[0004] In recent years, hydroxides have been considered to be excellent anode catalysts. However, the preparation of hydroxides mostly needs to be carried out under high temperature and high pressure liquid phase conditions, which is not conducive to large-scale preparation and difficult to industrialize.

[0005] Sulfides and phosphides can also show good catalytic water electrolysis oxygen activity, but this type of catalyst needs to be calcined at high temperature in a special atmosphere, and a sulfur source or phosphorus source is required to be continuously purged through the sample under the drive of an inert gas, resulting in a waste of raw materials. In addition, there are a large amount of toxic gases in the exhaust gas, which is also not suitable for large-scale preparation.

[0006] Metal oxides have the advantages of simple preparation methods and good catalyst stability, and are suitable for large-scale preparation. However, their intrinsic activity is slightly lower than that of the catalysts mentioned above. It is necessary to add multiple elements and adjust the appropriate proportions to effectively improve the intrinsic properties of the oxides. However, current technology makes it difficult to accurately control the proportions of elements in multi-element oxides. At the same time, the preparation method has a low utilization rate of raw materials, and the preparation process still needs to be optimized. Summary of the invention

[0007] In order to overcome the deficiencies of the prior art, the present invention provides a multi-element oxide electrode and a preparation method thereof, which can accurately control the element ratio in the multi-element oxide and has a very high raw material utilization rate.

[0008] The technical solution adopted by the present invention to solve its technical problem is: In a first aspect, the present application provides a method for preparing a multi-element oxide electrode, comprising the following steps: Using ethanol as solvent, preparing a reducing agent and at least two metal salts into a mixed solution; Placing the metal substrate in a heating environment, repeatedly dropping the mixed solution onto one side of the metal substrate and volatilizing it until half of the mixed solution is volatilized, and repeatedly dropping the mixed solution onto the other side of the metal substrate and volatilizing it until all of the mixed solution is volatilized; The metal substrate is calcined in a vacuum environment, and the multi-element oxide electrode is obtained after natural cooling.

[0009] The method for preparing a multi-oxide electrode provided in the present application comprises dropping a mixed solution onto a hot metal substrate, and then dropping another drop after it is completely volatilized or partially volatilized, so that the raw materials can be combined with the metal substrate with almost no excess and loss, and the influence of the different degrees of difficulty in combining different raw materials with the same substrate can be eliminated, which is conducive to the precise control of the proportion of elements in the multi-oxide.

[0010] Optionally, the metal substrate is a copper mesh, a nickel mesh, a copper foam or a nickel foam.

[0011] Optionally, the metal substrate is a copper mesh or a nickel mesh with a mesh size of 60 or more, and a wire diameter of 100 μm or more.

[0012] The metal substrate is made of copper mesh, nickel mesh, foam copper, and foam nickel, which is beneficial to increase the surface area and improve the bonding strength between the raw material and the metal substrate. When the metal substrate is a mesh structure, it is necessary to ensure that the mesh is small enough and the wire diameter is thick enough to prevent the droplets from passing through the metal substrate.

[0013] Optionally, when the mixed solution is dripped onto the metal substrate, the temperature of the heating environment is 80°C to 200°C, the volume of each drop is 50 μL to 500 μL, and the interval for repeated dripping at the same liquid contact point on the metal substrate is 1 min to 10 min.

[0014] The smaller the volume of liquid added each time and the more times the liquid is added, the more uniform the catalytic layer covering the metal substrate will be. When the metal substrate is placed in a heating environment, the temperature transferred to the metal substrate will decrease to a certain extent. The surface temperature of the metal substrate is slightly higher than 80 degrees. At this time, the amount of liquid added each time should be as small as possible, otherwise large drops of liquid will not be volatilized for a long time and will settle due to gravity and enter the metal substrate or pass through the metal substrate, causing raw material loss. When the area of ​​the metal substrate is large, it is necessary to appropriately increase the amount of liquid added each time and shorten the entire dropping time. At this time, the temperature of the heating plate needs to be greatly increased to promote the volatilization of the droplets, but the overall temperature should not exceed 200 degrees Celsius. The metal substrate is also prone to oxidation reactions at high temperatures, affecting the catalytic performance of the final product.

[0015] Optionally, the dropping height is 2 cm to 10 cm from the metal substrate.

[0016] If the distance is too large, the droplets will have too much impact on the metal substrate, which may cause the droplets to splash or pass through the mesh metal substrate. However, if the distance is too small, the heat of the metal substrate will be transferred to the outlet where the liquid is added, causing the liquid to evaporate quickly at the outlet, affecting the coverage on the metal substrate.

[0017] Optionally, the interval between adjacent liquid contact points is 0.5 cm to 2 cm, and the plurality of liquid contact points are arranged in a "H" shape.

[0018] Optionally, the step of preparing the mixed solution includes: adding the metal salt and the reducing agent into ethanol, and ultrasonically dissolving them to form a clear mixed solution; the preparation temperature is 20° C. to 30° C., and the ultrasonic time is 1 min to 10 min.

[0019] Optionally, during the calcination process, the heating rate is 2°C / min-10°C / min, the calcination temperature is 200°C-500°C, and the calcination time is 0.5h-3h.

[0020] Optionally, the reducing agent is citric acid, sodium citrate or ascorbic acid.

[0021] Optionally, the metal salt is a salt of at least two non-noble metals.

[0022] Optionally, the metal salt is at least two of iron salt, nickel salt and cobalt salt.

[0023] Optionally, the metal salt is a hydrated strong acid salt.

[0024] Optionally, the metal salt is selected from at least two of nickel chloride hexahydrate, cobalt chloride hexahydrate, and ferric chloride hexahydrate, and in the step of preparing the mixed solution, the molar ratio of the metal salt to ethanol is 1:1000-2000.

[0025] In a second aspect, the present application provides a multi-element oxide electrode, which is prepared by the multi-element oxide electrode preparation method described in the first aspect. The electrode has good catalytic activity and strong bonding with a metal substrate.

[0026] The beneficial effects of the present invention are as follows: the present invention can combine the raw materials on the metal substrate with almost no redundancy and loss, the raw material utilization rate is extremely high, the universality is wide, the influence of the different degrees of difficulty in combining different raw materials with the same substrate can be eliminated, the ratio and content of the metal salt attached to the metal substrate can be accurately controlled, and only simple calcination is required subsequently to form a compact multi-metal oxide electrode on the metal substrate.

[0027] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is one of the scanning electron microscope images of the final product obtained in Example 1.

[0029] Figure 2 This is the second scanning electron microscope image of the final product obtained in Example 1.

[0030] Figure 3 is the X-ray powder diffraction pattern of the final product of Example 1.

[0031] Figure 4 This is the elemental surface scan of the final product of Example 1.

[0032] Figure 5 It is a comparison chart of the electrochemical performance of the electrodes obtained in Example 1, Example 2 and Control Sample 1.

[0033] Figure 6 It is a comparison chart of the electrochemical performance of the electrodes obtained in Example 1 and Example 3.

[0034] Figure 7 It is a comparison chart of the electrochemical performance of the electrodes obtained from Example 1, Control Sample 2, and Control Sample 3.

[0035] Figure 8 It is a comparison chart of the electrochemical performance of the electrodes obtained in Example 4 and Example 5.

[0036] Fig. 9 It is a stability test diagram of the electrodes obtained in Example 4 and Example 5. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] It should be understood that, under the premise of no conflict, any and all embodiments of the present invention can be combined with the technical features in any other embodiment or multiple other embodiments to obtain another embodiment. The present invention includes such a combination to obtain another embodiment.

[0039] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.

[0040] Before the present application date, a hydrothermal method was generally used to grow a dense oxide catalyst layer in situ on a metal substrate, but the hydrothermal method requires a high temperature and high pressure environment, which is not conducive to subsequent amplification of production. Further, before the present application date, the preparation of oxide electrodes had low requirements for raw material utilization, and most of the metal salts remained in the solution, causing a lot of waste and increasing the preparation cost. It has been reported in the literature that Ni-based oxides have a significant effect on catalyzing the electrolysis of oxygen by water, and polybasic Ni-based oxides formed by doping other metal salts have a better catalytic effect, but the precise regulation and synthesis of polybasic Ni-based oxides has rarely been reported. A large part of the reason may be that the traditional hydrothermal method is difficult to control the metal ratio of metal oxides, which is not conducive to in-depth exploration of the intrinsic relationship between element ratio and catalytic activity.

[0041] Therefore, the applicant proposed a new method for preparing multi-element oxide metals for the catalytic electrode used at the anode end. The solvent is dripped and volatilized on the metal substrate to retain a layer of coating containing multi-metal salts, and then calcined at high temperature under vacuum conditions to obtain a multi-element oxide electrode. This scheme is suitable for preparing large-area electrodes, while improving the utilization rate of raw materials and reducing the preparation cost. In the future, large-area multi-element oxide electrodes can be industrially prepared by designing and manufacturing an electric drop gun, supplemented by a large-area heating device.

[0042] The present invention provides a method for preparing a multi-element oxide electrode, comprising the following steps: S1. Add a reducing agent and at least two metal salts into ethanol, and use ultrasound to promote dissolution to obtain a clear metal salt ethanol solution (i.e., a mixed solution).

[0043] S2. Place a metal substrate of appropriate area in a glass dish. After preheating the glass dish on a heating plate for a certain period of time, use a pipette to evenly drip the metal salt ethanol solution on the metal substrate. After each drip, the metal substrate needs to be kept in a heated environment to allow the ethanol to evaporate. After half of the mixed solution has been dripped, use tweezers to turn the metal sheet over, and repeat the above operation until the mixed solution has been dripped and evaporated.

[0044] S3. Place the metal substrate covered with the metal salt coating in a tube furnace, evacuate it, heat it to a suitable temperature at a certain heating rate and maintain it for a period of time. After the heating process is completed, cool it naturally. Wash the obtained sample with water and ethanol several times, and obtain the multi-oxide electrode after natural drying.

[0045] A certain ratio of metal salt ethanol solution is dripped onto the surface of a metal substrate, heated to volatilize the ethanol solvent, a metal salt coating is formed on the surface, and then calcined in a tubular furnace under vacuum conditions to form a dense multi-element oxide catalyst in situ. The metal elements in the oxide are in a relatively high valence state, which can reduce the energy barrier of oxidizing hydroxide ions and reduce the overpotential required for electrolysis of water. The catalyst has good catalytic activity and has a strong binding force with the metal substrate. The method can accurately control the metal content and ratio of the oxide, improve the utilization rate of raw materials, and enhance the activity and stability of the electrolysis of water and oxygen evolution at the anode.

[0046] In step S1, the plurality of metal salts include at least two of nickel salts, cobalt salts, and iron salts. The nickel salt may be nickel chloride hexahydrate or nickel nitrate hexahydrate, the cobalt salt may be cobalt chloride hexahydrate or cobalt nitrate hexahydrate, and the iron salt may be ferric chloride hexahydrate or ferric nitrate nonahydrate. Preferably, the nickel salt is nickel chloride hexahydrate, the cobalt salt is cobalt chloride hexahydrate, and the iron salt is ferric chloride hexahydrate. Nitrates are not preferred because they have certain explosion risks and are not as easily decomposed and volatilized as chlorides during the calcination process.

[0047] In step S1, the reducing agent is a small molecule containing hydroxyl group, which has weak reducing property and is slightly acidic, so as to avoid reaction with the metal salt to form precipitation, and can be citric acid or ascorbic acid. Preferably, the reducing agent is citric acid. The molar ratio of the total amount of the metal salt to the reducing agent can be 1:0.1-10, and preferably, the molar ratio of the total amount of the metal salt to the reducing agent is 1:0.5-2.

[0048] In step S1, the multi-metal salt mixture is an ethanol solution containing two or more non-precious metal salts. The non-precious metal salt can be a nickel salt, an iron salt or a cobalt salt. Further, the bimetallic salt mixture can be a mixture of a nickel salt and an iron salt, a mixture of a nickel salt and a cobalt salt, or a mixture of a cobalt salt and an iron salt. The trimetallic salt mixture is a mixture of a nickel salt, a cobalt salt and an iron salt.

[0049] Preferably, in the bimetallic salt mixture, the molar ratio of nickel salt to iron salt or cobalt salt is 1:0.1-10; more preferably, the molar ratio of nickel salt to iron salt or cobalt salt is 1:0.5-2. In the trimetallic salt mixture, the molar ratio of nickel salt, iron salt and cobalt salt is 1:0.1-10:0.1-10, preferably 1:1:1 or 0.02:0.14:0.14. Regardless of the bimetallic salt mixture or the trimetallic salt mixture, the ratio of the total amount of metal salt to the amount of ethanol is 1:1000-2000.

[0050] In step S2, the temperature of the heating plate can be 100°C to 200°C, and the preheating temperature can be 120°C to 180°C. Preferably, the temperature of the heating plate is 120°C to 160°C. While increasing the evaporation of the droplets, the oxidation of the metal substrate is avoided as much as possible. When the temperature of the heating plate is near 100 degrees Celsius, the temperatures of the glass dish and the metal substrate decrease in sequence. The temperature of the outermost layer of the metal substrate is slightly higher than 80 degrees. At this time, the amount of liquid dropped each time should be as small as possible. Otherwise, large droplets of liquid that have not been evaporated for a long time will settle due to gravity and contact the glass dish, resulting in loss of raw materials.

[0051] In step S2, the vertical distance from the lowest point of the pipette tip to the metal substrate is 2 cm to 10 cm. Preferably, the vertical distance is 2 cm to 5 cm.

[0052] In step S2, the dropping positions (or the liquid-receiving points on the metal substrate) during dropping can be spaced 0.5 cm to 2 cm apart. Preferably, the horizontal and vertical spacings are 0.5 cm to 1 cm, and the entire liquid array is arranged in a "ji" character shape. For example, starting from the upper left corner of the metal substrate, drop the liquid from left to right with a horizontal spacing of 0.5 cm to 2 cm. After dropping a horizontal row, move down with a vertical spacing of 0.5 cm to 2 cm and continue to drop from right to left. The entire liquid-receiving point array is arranged in a "ji" character shape. The spacing between the liquid-receiving points is positively correlated with the size of the droplets. The larger the droplets, the larger the spacing.

[0053] In step S2, the metal substrate is a copper-based substrate. The copper-based substrate can be copper foam or copper mesh. Preferably, the copper-based substrate is copper mesh. Copper mesh is inexpensive, has excellent electrical conductivity, and a relatively large specific surface area, and is expected to replace nickel mesh as a new generation of electrode substrate. Moreover, the metal salt mainly from the eighth subgroup is used in the present invention. If a nickel-based substrate is used, it will affect the elemental analysis results of the catalyst. It is more suitable to use copper mesh. The area of the metal substrate can be 2 cm * 2 cm to 20 cm * 20 cm. Preferably, the metal substrate of 5 cm * 5 cm is used in the examples of this application. The mesh number is 60, and the wire diameter is 250 microns. Correspondingly, the total volume of the solution is 10 ml to 50 ml.

[0054] In step S3, the calcination temperature is 200°C to 500°C, preferably 200°C to 400°C. The temperature rising rate is 2 degrees Celsius per minute to 10 degrees Celsius per minute, and the holding time is 0.5 hour to 3 hours, preferably 0.5 hour to 2 hours. The calcination atmosphere can be a vacuum environment or an inert atmosphere. The inert atmosphere can be an argon atmosphere, etc. Preferably, the present invention performs calcination in a vacuum environment, which saves costs and is easier to operate. If the temperature is too high, the metal substrate will become brittle and unusable. If the temperature rising rate is too fast, the coating will react sharply and form cracks.

[0055] Example 1 Cut a 5*5cm copper mesh and place it in a glass dish. Place the glass dish on a heating plate and preheat at 150℃ for 5 minutes. The metal salt preparation process is as follows: 0.1mmol each of nickel chloride hexahydrate, ferric chloride hexahydrate and cobalt chloride hexahydrate and 1mmol of citric acid are added to 20ml of ethanol and ultrasonicated for 5 minutes to obtain a clear solution. Use a pipette to evenly add 200μL of solution on the copper mesh each time. After heating for 1 minute, continue to add until half of the solution has been added. Turn the copper mesh over with tweezers and repeat the above operation until all the solution has been added.

[0056] The copper mesh covered with the metal salt coating was transferred to a tube furnace. After evacuation for half an hour, the temperature was raised from room temperature to 300°C at a rate of 10°C per minute and kept at that temperature for 1 hour. After the end of the heat preservation, the copper mesh was naturally cooled. The copper mesh was cleaned with pure water and ethanol and dried naturally to obtain a NiCoFe electrode. The electrode was observed under an electron microscope. Figure 1 and Figure 2 As shown, from Figure 1 and Figure 2 It can be seen that the copper mesh is loaded with a dense coating. The X-ray powder diffraction pattern of the final product of Example 1 is as follows Figure 3 As shown in the figure, the coating has almost no peaks. It may be that the peak intensity of the copper mesh substrate is too strong to cover the signal of the coating. The element mapping analysis (element mapping) of the electrode is performed, and the results are as follows Figure 4 ( Figure 4 As shown in the first picture "ch1" in the figure, which indicates the original SEM image, it can be found that Ni, Co, Fe, and O elements are evenly distributed (due to the non-absolute vacuum test conditions, there is a certain inaccuracy in the oxygen content).

[0057] Example 2 Cut three 5*5cm copper meshes and place them in a glass dish. Place the glass dish on a heating plate and preheat at 150℃ for 5 minutes. The preparation process of three groups of solutions containing two metal salts is as follows: Each group selects two salts from nickel chloride hexahydrate, ferric chloride hexahydrate and cobalt chloride hexahydrate, each 0.15mmol, and then adds them together with 1mmol of citric acid to 20ml ethanol, and ultrasonicates for 5 minutes to obtain a clear solution. Each group uses a pipette to evenly add a total of 200μL of solution on the copper mesh each time. After heating for 1 minute, continue to add until half of the solution has been added. Turn the copper mesh over with tweezers and repeat the above operation until all the solution has been added.

[0058] The remaining operations (calcination, cleaning, and drying) are the same as those in Example 1, and a NiCo electrode, a NiFe electrode, and a CoFe electrode can be obtained.

[0059] Example 3 Cut three 5*5cm copper meshes and place them in a glass dish. Place the glass dish on a heating plate and preheat at 150℃ for 5 minutes. Prepare three groups of solutions containing three metal salts: 0.02mmol nickel chloride hexahydrate, 0.14mmol ferric chloride hexahydrate, 0.14mmol cobalt chloride hexahydrate and 1mmol citric acid; 0.14mmol nickel chloride hexahydrate, 0.02mmol ferric chloride hexahydrate, 0.14mmol cobalt chloride hexahydrate and 1mmol citric acid; 0.14mmol nickel chloride hexahydrate, 0.14mmol ferric chloride hexahydrate, 0.02mmol cobalt chloride hexahydrate, and add them to 20ml ethanol together with 1mmol citric acid, and ultrasonicate for 5 minutes to obtain a clear solution. Each group uses a pipette to evenly add a total of 200μL of solution on the copper mesh each time. After heating for 1 minute, continue to add until half of the solution has been added. Use tweezers to turn the copper mesh over and repeat the above operation until all the solution has been added.

[0060] The remaining operations are the same as in Example 1, and Ni 0.14 CoFe electrode, NiCo 0.14 Fe electrode, NiCoFe 0.14 electrode.

[0061] Example 4 Except that the metal substrate is replaced with a nickel mesh, the steps are the same as those in Example 1. A NiCoFe / Ni mesh electrode can be obtained.

[0062] Example 5 Except that the amount of metal salt added is changed to 0.14 mmol nickel chloride hexahydrate, 0.14 mmol ferric chloride hexahydrate, and 0.02 mmol cobalt chloride hexahydrate, the other steps are the same as those in Example 4. NiCo 0.14 Fe / Ni mesh electrode.

[0063] Control sample 1 Cut a 5*5cm copper mesh and place it in a glass dish. Place the glass dish on a heating plate and preheat at 150℃ for 5 minutes. The metal salt preparation process is as follows: 0.3mmol of one of nickel chloride hexahydrate, cobalt chloride hexahydrate and ferric chloride hexahydrate and 1mmol of citric acid are added to 20ml of ethanol and ultrasonicated for 5 minutes to obtain a clear solution. Use a pipette to evenly add a total of 200μL of solution on the copper mesh each time. After heating for 1 minute, continue to add until half of the solution has been added. Turn the copper mesh over with tweezers and repeat the above operation until all the solution has been added.

[0064] The remaining operations are the same as those in Example 1, and a Ni electrode, a Co electrode and a Fe electrode can be obtained.

[0065] Control sample 2 The ternary oxide electrodes were prepared using a conventional hydrothermal method.

[0066] Cut a 2cm*5cm copper mesh and put it into a 50ml polytetrafluoroethylene liner. Dissolve 0.1mmol each of nickel chloride hexahydrate, ferric chloride hexahydrate and cobalt chloride hexahydrate and 1mmol of citric acid in 20ml of deionized water and transfer them to the polytetrafluoroethylene liner containing the copper mesh. After sealing the hydrothermal reactor shell, put it in an oven and heat it to 100 degrees Celsius for 10 hours. After the reaction is completed, cool it naturally, take out the sample, wash it with water and ethanol, and dry it naturally to obtain the NiCoFe-SR control sample.

[0067] Control sample 3 The ternary oxide electrodes were prepared using a spray coating method.

[0068] Cut a 5cm*5cm copper mesh and place it in a glass dish. Place the glass dish on a heating plate and preheat at 150℃ for 5 minutes. The metal salt preparation process is as follows: 0.1mmol each of nickel chloride hexahydrate, ferric chloride hexahydrate and cobalt chloride hexahydrate and 1mmol of citric acid are added to 20ml of ethanol and ultrasonicated for 5 minutes to obtain a clear solution. Use a spray pen to continuously spray the solution on the surface of the copper mesh until half of the solution is sprayed. Turn the copper mesh over with tweezers and repeat the above operation until all the solution is sprayed.

[0069] The remaining operations (calcination, washing, drying) are the same as those in Example 1.

[0070] The electrodes prepared in Example 1, Example 2 and Example 3 were subjected to EDS element analysis. The results are shown in Table 1.

[0071] Table 1 sample Ni Co Fe Example 2 NiCo 51.7% 48.2% Example 2 NiFe 49.7% 50.2% Example 2 CoFe 48.6% 51.3% Example 1 NiCoFe 32.7% 33.3% 33.9% <![CDATA[Example 3 Ni 0.14 CoFe]]> 2.2% 53.7% 44.4% <![CDATA[Example 3 NiCo 0.14 Fe]]> 46.6% 4.0% 49.1% <![CDATA[Example 3 NiCoFe 0.14 > 47.4% 49.6 6.2% From Table 1 (due to the influence of rounding, trace impurities, etc., the sum of the data may not be equal to 100%), it can be seen that the method of the present application can basically accurately control the proportion of metal elements coated on the copper mesh, and has a certain universality.

[0072] The NiCoFe electrode of Example 1, the NiCo electrode of Example 2, the NiFe electrode of Example 2, the CoFe electrode of Example 2, and the Ni 014 CoFe electrode, Example 3 NiCo 0.14 Fe electrode, Example 3 NiCoFe 0.14 Electrode, Example 4 NiCoFe / Ni mesh electrode, Example 5 NiCo 0.14 The electrolytic water oxygen evolution activity of the Fe / Ni mesh electrode, control sample 1 Ni electrode, control sample 1 Co electrode, control sample 1 Fe electrode, control sample 2 NiCoFe-SR electrode, and control sample 3 electrodes was tested, and the results were shown in the linear sweep voltammetric curve ( Figures 5 to 8) display. Among them, the electrochemical test conditions are: 25°C, 1mol / L KOH. The working electrode is the electrode prepared in the embodiment, the reference electrode is Hg / HgO, and the counter electrode is a platinum electrode. First, a cyclic voltammetry test is performed on the working electrode to achieve the activation effect. The scanning range is 0.8V~1.7V vs RHE, and the scanning rate is 0.1V / s. The test is stopped when the electrode is stable. Then the electrochemical activity of the electrode is tested using linear scanning voltammetry. The scanning range is 1.2V~1.7V vs RHE, and the scanning rate is 5mV / s.

[0073] The electrolytic water oxygen evolution activity test results of the comparative example 1, example 2 and control sample 1 are as follows: Figure 5 As shown in the figure, the general performance ranking is that the ternary electrode is better than the binary electrode, and the binary electrode is better than the unit electrode. The NiCoFe electrode only needs 408mV to reach 50mAcm -2 .

[0074] Comparing the test results of the electrolytic water oxygen evolution activity of Example 1 and Example 3, as shown in Figure 6 As shown, the NiCo of Example 3 0.14 The Fe electrode is superior to the NiCoFe electrode in Example 1, and only 373 mV overpotential is required to reach 50 mA cm -2 , indicating that further optimizing the element ratio of the ternary electrode can further improve the catalytic performance of the electrode.

[0075] The electrolytic water oxygen evolution activity test results of the comparative example 1, the control sample 2 and the control sample 3 are as follows: Figure 7 As shown, Example 1 is called the drip coating method, Control Sample 2 is called the hydrothermal method, and Control Sample 3 is called the spray coating method. The results show that the performance of the drip coating method is slightly better than that of the spray coating method, which may be because the drip coating method can better retain the raw materials on the metal substrate. On the other hand, the spray coating method requires professional spraying equipment, and the equipment has general corrosion resistance to metal salt solutions. In addition, the spray coating method takes a long time to complete the spraying, which easily causes corrosion and pore blockage of the spray gun. The electrode made by the hydrothermal method has the worst performance, which may be because the amount of in-situ growth on the substrate is far less than the amount of raw material added, and the catalytic sites are far less than the drip coating method of this application.

[0076] Comparative Example 4 and Example 5 electrolysis water oxygen evolution activity test results, such as Figure 8 As shown, NiCo 0.14 The Fe / Ni mesh only needs 348 mV overpotential to reach 50 mA cm -2 This indicates that replacing a more suitable substrate can further improve the catalytic activity of the obtained multi-oxide electrode.

[0077] The stability test of the electrodes of Example 4 and Example 5 was performed under constant current. The results are as follows: Fig. 9As shown, it can be seen that the electrode performance of the two embodiments is basically stable within 25 hours. The constant current test conditions are: 25°C, 1 mol / L KOH, the counter electrode is a platinum sheet, and the current is set to 100 mA.

[0078] The present application embodiment provides a method for preparing an electrode that is simple to operate, has high raw material utilization, and is widely applicable by optimizing the ratio and dosage between the metal salt, the reducing agent, and the ethanol in the salt solution. The ratio and content of the metal salt attached to the metal substrate can be accurately regulated. Subsequently, a compact multi-metal oxide electrode can be formed on the metal substrate by simple high-temperature heating. The high-valent metal oxide on the surface of the catalytic electrode can effectively reduce the reaction activation energy and increase the water electrolysis reaction rate. Moreover, the catalytic layer has a strong binding force with the metal substrate, and the multi-metal oxide electrode can work for a long time under high current conditions. The electrode prepared by the preparation method of the present application has a catalytic water electrolysis oxygen activity that is better than the control sample prepared by a single metal salt, and is also better than the control sample prepared by a conventional hydrothermal method and a spraying method, and can work for a long time under high current density. This scheme has great application prospects, and the method is expected to be applied to the preparation of other electrode materials.

[0079] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0080] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a multi-element oxide electrode, characterized in that: The following steps are involved: Using ethanol as solvent, preparing a reducing agent and at least two metal salts into a mixed solution; Placing the metal substrate in a heating environment, repeatedly dropping the mixed solution onto one side of the metal substrate and volatilizing it until half of the mixed solution is volatilized, and repeatedly dropping the mixed solution onto the other side of the metal substrate and volatilizing it until all of the mixed solution is volatilized; The metal substrate is calcined in a vacuum environment, and the multi-element oxide electrode is obtained after natural cooling.

2. The method for preparing a multi-element oxide electrode according to claim 1, characterized in that: The metal substrate is a copper mesh, a nickel mesh, a foam copper or a foam nickel.

3. The method for preparing a multi-element oxide electrode according to claim 2, characterized in that: The metal substrate is a copper mesh or a nickel mesh with a mesh size of 60 or more, and a wire diameter of 100 μm or more.

4. The method for preparing a multi-element oxide electrode according to claim 1, characterized in that: When the mixed solution is dripped onto the metal substrate, the temperature of the heating environment is 80°C to 200°C, the volume of each drop is 50 μL to 500 μL, and the interval for repeated dripping at the same liquid contact point on the metal substrate is 1 min to 10 min.

5. The method for preparing a multi-element oxide electrode according to claim 4, characterized in that: The drop height is 2 cm to 10 cm from the metal substrate.

6. The method for preparing a multi-element oxide electrode according to claim 4, characterized in that: The adjacent liquid contact points are spaced 0.5 cm to 2 cm apart, and the plurality of liquid contact points are arranged in a "H" shape.

7. The method for preparing a multi-element oxide electrode according to claim 1, characterized in that: The step of preparing the mixed solution comprises: adding the metal salt and the reducing agent into ethanol, and ultrasonically dissolving to form a clarified mixed solution; the preparation temperature is 20° C. to 30° C., and the ultrasonic time is 1 min to 10 min.

8. The method for preparing a multi-element oxide electrode according to claim 1, characterized in that: During the calcination process, the heating rate is 2°C / min-10°C / min, the calcination temperature is 200°C-500°C, and the calcination time is 0.5h-3h.

9. The method for preparing a multi-element oxide electrode according to claim 1, characterized in that: The metal salt is selected from at least two of nickel chloride hexahydrate, cobalt chloride hexahydrate, and ferric chloride hexahydrate. In the step of preparing the mixed solution, the molar ratio of the metal salt to ethanol is 1:1000-2000.

10. A multi-element oxide electrode, characterized in that: The multi-oxide electrode is prepared by the method for preparing the multi-oxide electrode according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of CuCoNiMoFe multi-element oxide electrolyzed water catalyst

    CN116145177A

  • Batch preparation method of NiFe-based composite oxygen evolution anode

    CN117107286A

  • Amphoteric metal oxide doped nickel-cobalt oxide material as well as preparation method and application thereof

    CN117661014A