Modified short carbon fiber as well as preparation method and application thereof
By pre-oxidizing, low-temperature carbonization, high-temperature carbonization and surface oxidation treatment of carbon fibers, and cutting them in water-soluble polymer bundling agents, the problem of chopped carbon fibers being difficult to disperse in water is solved, and the performance of carbon fiber paper is improved. It is suitable for Proton exchange membrane fuel cell gas diffusion layer.
Patent Information
- Application Number
- CN202310555534.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The existing chopped carbon fibers are difficult to disperse evenly in water, resulting in poor mechanical properties of carbon fiber papers. In the prior art, removing the sizing agent and then performing surface treatments are time-consuming and energy-consuming, and the effect is not ideal.
By pre-oxidizing, low-temperature carbonization, and high-temperature carbonization, and surface oxidation treatment, and soaking it in a water-soluble polymer clustering agent solution to dry and chop, chopping carbon fibers to improve its dispersion in water and Combining ability.
It significantly improves the dispersion effect of modified chopped carbon fiber in water, simplifies the production process, improves the mechanical strength and conductive properties of carbon fiber paper, and meets the requirements of the gas diffusion layer of the proton exchange membrane fuel cell.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber, and specifically relates to a modified short-cut carbon fiber and a preparation method thereof, and the modified short-cut carbon fiber is used for a gas diffusion layer of a proton exchange membrane fuel cell. Background Art
[0002] In recent years, energy transformation and green and low-carbon development have become an unstoppable global trend. With the continuous development of the low-carbon economy, all countries have regarded hydrogen energy as a major energy strategic choice and a priority research field. As one of the most important hydrogen energy conversion devices, proton exchange membrane fuel cells (PEMFC) have received widespread attention. As a key material for PEMFC, the gas diffusion layer (GDL) plays an important role in the operation of the battery, including: water and gas transmission channel, electricity and heat transfer medium, and support and stability of the entire electrode. The gas diffusion layer is usually composed of a base layer and a microporous layer. Carbon fiber paper is currently the most widely used gas diffusion layer base material.
[0003] Carbon fiber paper is mainly prepared by wet process, that is, short-cut carbon fiber is evenly dispersed in water, and then it is prepared by a series of processes such as papermaking, resin impregnation, curing and forming, and finally carbonization, graphitization, etc. Due to the small number of surface active groups, strong hydrophobicity and weak bonding between fibers, short-cut carbon fiber is difficult to disperse evenly in water, and the mechanical properties of the carbon fiber paper are poor, which is also the main problem faced by the current wet process.
[0004] The existing preparation of chopped carbon fibers is obtained by chopping carbon fibers containing epoxy resin sizing agents. They have good bundling properties but are difficult to disperse in water (China Papermaking, 2019, 38(4): 41-44; Chinese Patent CN107217491A). Although commercialized carbon fibers are also surface treated, they are not designed to improve hydrophilicity and are not suitable for papermaking. Therefore, the existing technical solutions for carbon fiber paper are that the chopped carbon fibers are first subjected to high temperature or organic solvents to remove the sizing agent and then re-surface treated to improve their hydrophilicity and dispersibility, which is time-consuming and energy-consuming and the effect is not ideal. Summary of the invention
[0005] In response to the above technical problems, the present invention provides a modified chopped carbon fiber and a method for preparing the modified chopped carbon fiber, and uses the modified chopped carbon fiber for the gas diffusion layer of a proton exchange membrane fuel cell, which can solve the problem that carbon fiber is difficult to disperse evenly in water and improve the performance of carbon fiber paper.
[0006] One of the purposes of the present invention is to provide a method for preparing modified chopped carbon fibers, comprising: subjecting carbon fibers to surface oxidation treatment, modification with a sizing agent, drying, and chopping to obtain the modified chopped carbon fibers.
[0007] According to some embodiments of the present invention, the carbon fiber is not particularly limited, and commonly used carbon fiber materials in the art may be selected. For example, the carbon fiber is selected from at least one of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, and viscose-based carbon fiber.
[0008] According to some embodiments of the present invention, the sizing agent is selected from water-soluble high molecular polymers, preferably at least one selected from polyvinyl alcohol, methyl cellulose, sodium hydroxymethyl cellulose, hydroxyethyl cellulose, and water-based polyurethane.
[0009] According to some embodiments of the present invention, the preparation method specifically comprises the following steps:
[0010] (1) pre-oxidizing, low-temperature carbonizing, and high-temperature carbonizing the carbon fiber precursor to obtain carbon fiber;
[0011] (2) performing surface oxidation treatment on the carbon fiber obtained in step (1);
[0012] (3) Immersing the oxidized carbon fiber in a sizing agent solution, drying, and chopping to obtain the modified chopped carbon fiber.
[0013] In the above preparation method, the pre-oxidation, low-temperature carbonization and high-temperature carbonization processes in the step (1) can adopt the operating processes commonly used in the art. Preferably, the pre-oxidation conditions are: the pre-oxidation atmosphere is air, and the pre-oxidation is carried out at 180-330°C for 20-100 min, preferably at 200-280°C for 30-90 min; the low-temperature carbonization conditions are: the low-temperature carbonization atmosphere is nitrogen, and the carbonization is carried out at 300-900°C for 1-3 min, preferably at 350-850°C for 1.5-2.5 min; the high-temperature carbonization conditions are: the high-temperature carbonization atmosphere is nitrogen, and the carbonization is carried out at 900-1500°C for 1-3 min, preferably at 1000-1400°C for 1.5-2.5 min.
[0014] In the above preparation method, the surface oxidation treatment is selected from one of electrochemical anodization, liquid phase oxidation, and gas phase oxidation. The conditions of the electrochemical anodization are: the electrolyte concentration is 0.1-3.0 mol / L, the electrolyte is selected from at least one of ammonium bicarbonate, diammonium phosphate, ammonium carbonate, sodium phosphate, sodium hydroxide, and sulfuric acid, and the current density is 0.1-2.0 mA / cm 2, the electrolysis time is 30 to 120 seconds; the conditions for the liquid phase oxidation are: the liquid phase medium is selected from a solution of at least one of nitric acid, acidic potassium dichromate, sodium hypochlorite, hydrogen peroxide, and potassium persulfate, the concentration of the liquid phase medium is 0.5 to 5 mol / L, the temperature is 30 to 80°C, and the time is 1 to 3 hours; the conditions for the gas phase oxidation are: in a mixed atmosphere of air and ozone, the treatment temperature is 150 to 450°C, and the treatment time is 60 to 240 seconds; preferably, in the mixed atmosphere, the volume percentage concentration of ozone is 0.5 to 5.0%.
[0015] In the above preparation method, in the step (3): the mass percentage concentration of the sizing agent in the sizing agent solution is 0.5-10%, for example, it can be any value among 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or the range between any two values. Preferably, the mass percentage concentration of the sizing agent in the sizing agent solution is 1-5%.
[0016] In the above preparation method, the drying in step (3) can adopt the drying equipment and drying conditions commonly used in the art, for example, the following process can be adopted: the drying conditions are 80-150° C. for 0.5-3 h, preferably 100-120° C. for 1-2 h.
[0017] The second object of the present invention is to provide a modified chopped carbon fiber prepared by the above-mentioned preparation method. Preferably, the obtained modified chopped carbon fiber comprises carbon fiber and a sizing agent on the surface of the carbon fiber.
[0018] According to some embodiments of the present invention,
[0019] The total fineness of the modified chopped carbon fiber is 3000-36000 dtex, for example, it can be any value of 3000, 5000, 8000, 10000, 12000, 15000, 18000, 20000, 22000, 25000, 30000, 32000, 36000 or a range between any two values. Preferably, the total fineness of the modified chopped carbon fiber is 10000-30000 dtex;
[0020] The aspect ratio of the modified chopped carbon fiber is 500-6000, for example, it can be any value of 500, 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000, 3500, 4000, 4500, 5000, 5500, 6000 or a range between any two values. Preferably, the aspect ratio of the modified chopped carbon fiber is 1000-3000;
[0021] The surface carbon content of the modified short chopped carbon fiber is 50-95%, for example, it can be any value of 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or a range between any two values. Preferably, the surface carbon content of the modified short chopped carbon fiber is 60-80%;
[0022] The surface energy of the modified chopped carbon fiber is 50 to 110 mJ / m 2 , for example, it can be any value among 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110 or a range between any two values. Preferably, the surface energy of the modified chopped carbon fiber is 80 to 100 mJ / m 2 ;
[0023] The dispersion time of the modified chopped carbon fiber in water is 5 to 15 seconds, for example, it can be any value among 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or a range between any two values;
[0024] Taking the total mass of the modified chopped carbon fiber as 100%, the content of the sizing agent on the surface of the carbon fiber is 0.1-5%. For example, it can be any value among 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or the range between any two values. Preferably, taking the total mass of the modified chopped carbon fiber as 100%, the content of the sizing agent on the surface of the carbon fiber is 0.5-3%.
[0025] The third object of the present invention is to provide an application of the modified chopped carbon fiber in a gas diffusion layer of a proton exchange membrane fuel cell.
[0026] The present invention pre-oxidizes carbon fiber precursor, performs low-temperature carbonization and high-temperature carbonization, and then performs specific surface treatment and bundling agent treatment to obtain modified short-cut carbon fiber. The present invention provides a modified short-cut carbon fiber for a proton exchange membrane fuel cell gas diffusion layer and a preparation method of the modified short-cut carbon fiber, which can solve the problem that carbon fiber is difficult to disperse uniformly in water and improve the performance of carbon fiber paper.
[0027] The present invention first performs corresponding surface treatment on the carbon fiber, and then modifies it through a specific sizing agent. On the one hand, the surface properties of the carbon fiber can be changed to improve its dispersibility in water and the bonding ability between fibers; on the other hand, the process of removing the pulp and then treating and modifying the chopped carbon fiber in the process of preparing the carbon fiber paper is omitted, the steps are simplified, and the production efficiency is improved. The modified chopped carbon fiber obtained by the present invention can well meet the requirements of the gas diffusion layer of the proton exchange membrane fuel cell for the raw material chopped carbon fiber, and the dispersion effect of the modified chopped carbon fiber in water is significantly improved, so the thickness of the prepared carbon fiber paper is more uniform, thereby greatly improving the mechanical strength and conductive properties of the product. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0029] The test instruments and test conditions used in the examples are as follows:
[0030] The surface carbon content was measured by X-ray photoelectron spectroscopy.
[0031] The surface energy was tested by inverse gas chromatography surface energy analyzer.
[0032] The sizing agent content is tested using "GB / T29761-2022 Determination of carbon fiber sizing agent content".
[0033] The carbon fiber fineness is tested using the "GB / T14343-2008 Test method for linear density of chemical fiber filaments".
[0034] The aspect ratio of carbon fiber is tested using "GB\T29762-2013 Determination of carbon fiber diameter and cross-sectional area".
[0035] The dispersion time was tested using the method in patent CN108018719A.
[0036] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0037] [Example 1]
[0038] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundling treatment is carried out, the bundling agent is polyvinyl alcohol aqueous solution, the concentration is 2%. After that, it is dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000dtex, the bundling agent content is 1.2%, the aspect ratio is 1000, the surface carbon content is 75%, and the surface energy is 82mJ / m 2 , dispersion time in water is 13s.
[0039] [Example 2]
[0040] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to liquid phase oxidation surface treatment, 3 mol / L nitric acid aqueous solution, soaked at 60°C for 2 hours, washed and dried. Then, a bundling treatment was carried out, and the bundling agent was a polyvinyl alcohol aqueous solution with a concentration of 2%, then dried at 110°C for 1h and chopped to obtain modified chopped carbon fiber. The total fineness of the modified chopped carbon fiber was 10000 dtex, the bundling agent content was 1.3%, the aspect ratio was 1000, the surface carbon content was 67%, and the surface energy was 93mJ / m 2 , dispersion time in water is 7s.
[0041] [Example 3]
[0042] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to gas phase oxidation surface treatment, with a mixed atmosphere of air and ozone, an ozone concentration of 2% (v%), a treatment temperature of 250°C, and a treatment time of 150s. Then, a bundling treatment was carried out, with a bundling agent of 2% polyvinyl alcohol aqueous solution, followed by drying at 110°C for 1h and chopped to obtain modified chopped carbon fiber. The total fineness of the modified chopped carbon fiber was 10000 dtex, the bundling agent content was 1.2%, the aspect ratio was 1000, the surface carbon content was 63%, and the surface energy was 95 mJ / m 2 , dispersion time in water is 9s.
[0043] [Example 4]
[0044] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundling treatment is carried out, the bundling agent is polyvinyl alcohol aqueous solution, the concentration is 5%. After that, it is dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000dtex, the bundling agent content is 2.9%, the aspect ratio is 1000, the surface carbon content is 73%, and the surface energy is 80mJ / m 2 , dispersion time in water is 15s.
[0045] [Example 5]
[0046] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundling treatment is carried out, the bundling agent is polyvinyl alcohol aqueous solution, the concentration is 1%. After that, it is dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000dtex, the bundling agent content is 0.6%, the aspect ratio is 1000, the surface carbon content is 74%, and the surface energy is 81mJ / m 2 , dispersion time in water is 11s.
[0047] [Example 6]
[0048] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then the low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then the high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 1.0 mA / cm 2 , electrolysis time 60s. Then the bundling treatment is carried out, the bundling agent is polyvinyl alcohol aqueous solution, the concentration is 2%. After that, it is dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000dtex, the bundling agent content is 1.2%, the aspect ratio is 1000, the surface carbon content is 69%, and the surface energy is 87mJ / m 2 , dispersion time in water is 9s.
[0049] [Example 7]
[0050] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to liquid phase oxidation surface treatment, 5 mol / L nitric acid aqueous solution, soaked at 60°C for 2 hours, washed and dried. Then, a bundling treatment was carried out, and the bundling agent was a polyvinyl alcohol aqueous solution with a concentration of 2%, then dried at 110°C for 1h and chopped to obtain modified chopped carbon fiber. The total fineness of the modified chopped carbon fiber was 10000 dtex, the bundling agent content was 1.4%, the aspect ratio was 1000, the surface carbon content was 63%, and the surface energy was 97 mJ / m 2 , dispersion time in water is 6s.
[0051] [Comparative Example 1]
[0052] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundle treatment is carried out, using the traditional epoxy resin sizing agent with a concentration of 2%, then dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000dtex, the bundling agent content is 1.3%, the aspect ratio is 1000, the surface carbon content is 81%, and the surface energy is 63mJ / m 2 , the dispersion time in water is more than 5 minutes and it cannot be completely dispersed.
[0053] [Comparative Example 2]
[0054] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to liquid phase oxidation surface treatment, 3 mol / L nitric acid aqueous solution, soaked at 60°C for 2 hours, washed and dried. Then, a bundling treatment was carried out, using a traditional epoxy resin sizing agent with a concentration of 2%, then dried at 110°C for 1h and chopped to obtain modified chopped carbon fiber. The total fineness of the modified chopped carbon fiber is 10000 dtex, the bundling agent content is 1.5%, the aspect ratio is 1000, the surface carbon content is 83%, and the surface energy is 71mJ / m 2 , the dispersion time in water is more than 5 minutes and it cannot be completely dispersed.
[0055] [Comparative Example 3]
[0056] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 minutes through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 minutes through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 minutes through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to gas phase oxidation surface treatment, with a mixed atmosphere of air and ozone, an ozone concentration of 2% (v%), a treatment temperature of 250°C, and a treatment time of 150s. Then, a bundling treatment was carried out, using a traditional epoxy resin sizing agent with a concentration of 2%, and then dried at 110°C for 1h and chopped to obtain modified chopped carbon fiber. The total fineness of the modified short-cut carbon fiber is 10000 dtex, the sizing agent content is 1.4%, the aspect ratio is 1000, the surface carbon content is 76%, and the surface energy is 73mJ / m 2 , the dispersion time in water is more than 5 minutes and it cannot be completely dispersed.
[0057] [Comparative Example 4]
[0058] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundling treatment was carried out, the bundling agent was polyacrylamide aqueous solution, the concentration was 2%, then dried at 110℃ for 1h, and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber was 10000dtex, the bundling agent content was 1.7%, the aspect ratio was 1000, the surface carbon content was 81%, and the surface energy was 67mJ / m 2 , dispersion time in water is 97s.
[0059] [Comparative Example 5]
[0060] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 min through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 min through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 min through 3 stages of gradient heating, to obtain carbon fiber. The carbon fiber was subjected to electrochemical surface treatment, with the electrolyte being 0.5 mol / L NH4HCO3 and the current density being 0.5 mA / cm 2 , electrolysis time 60s. Then the bundling treatment was carried out, the bundling agent was polyvinyl alcohol aqueous solution, the concentration was 7%, then dried at 110℃ for 1h and chopped to obtain modified short-cut carbon fiber. The total fineness of the modified short-cut carbon fiber was 10000dtex, the bundling agent content was 2.3%, the aspect ratio was 1000, the surface carbon content was 77%, and the surface energy was 72mJ / m 2 , dispersion time in water is 135s.
[0061] [Comparative Example 6]
[0062] The polyacrylonitrile precursor was pre-oxidized, carbonized at low temperature and carbonized at high temperature. The pre-oxidation was first carried out in an air atmosphere, with a temperature range of 200-280°C and a time of 90 minutes through 6 stages of gradient heating; then low-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 350-850°C and a time of 2 minutes through 3 stages of gradient heating; then high-temperature carbonization was carried out in a nitrogen atmosphere, with a temperature range of 1000-1400°C and a time of 2 minutes through 3 stages of gradient heating, to obtain carbon fiber. Then, a bundling treatment was carried out, and the bundling agent was a polyvinyl alcohol aqueous solution with a concentration of 2%. After that, it was dried at 110°C for 1 hour and chopped to obtain modified chopped carbon fiber. The total fineness of the modified chopped carbon fiber is 10000 dtex, the bundling agent content is 1.0%, the aspect ratio is 1000, the surface carbon content is 93%, and the surface energy is 43mJ / m 2 , dispersion time in water is 196s.
[0063] Obviously, by adopting the technical scheme of the present invention, the polyacrylonitrile precursor is pre-oxidized, low-temperature carbonized and high-temperature carbonized, and then subjected to specific surface treatment and bundling agent treatment, and then chopped carbon fibers are obtained, which solves the problem that carbon fibers are difficult to disperse evenly in water, and can be used for the preparation of gas diffusion layers of proton exchange membrane fuel cells.
Claims
1. A method for preparing modified chopped carbon fiber, comprising: The carbon fiber is subjected to surface oxidation treatment, modified by a sizing agent, dried, and chopped to obtain the modified chopped carbon fiber.
2. The preparation method according to claim 1, characterized in that: The carbon fiber is selected from at least one of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, and viscose-based carbon fiber; and / or, The sizing agent is selected from water-soluble high molecular polymers, preferably at least one selected from polyvinyl alcohol, methyl cellulose, sodium hydroxymethyl cellulose, hydroxyethyl cellulose, and water-based polyurethane.
3. The preparation method according to claim 1 or 2, characterized in that: The preparation method specifically comprises the following steps: (1) pre-oxidizing, low-temperature carbonizing, and high-temperature carbonizing the carbon fiber precursor to obtain carbon fiber; (2) performing surface oxidation treatment on the carbon fiber obtained in step (1); (3) Immersing the oxidized carbon fiber in a sizing agent solution, drying, and chopping to obtain the modified chopped carbon fiber.
4. The preparation method according to claim 3, characterized in that: In the step (1): The pre-oxidation conditions are: 180-330° C. for 20-100 min, preferably 200-280° C. for 30-90 min; and / or, The low temperature carbonization conditions are: carbonization at 300-900°C for 1-3 min, preferably carbonization at 350-850°C for 1.5-2.5 min; and / or, The high temperature carbonization conditions are: carbonization at 900-1500° C. for 1-3 min, preferably carbonization at 1000-1400° C. for 1.5-2.5 min.
5. The preparation method according to claim 3, characterized in that: The surface oxidation treatment in step (2) is selected from electrochemical anodization, liquid phase oxidation, and gas phase oxidation.
6. The preparation method according to claim 5, characterized in that: The conditions of the electrochemical anodization are: the electrolyte concentration is 0.1-3.0 mol / L, the electrolyte is selected from at least one of ammonium bicarbonate, diammonium phosphate, ammonium carbonate, sodium phosphate, sodium hydroxide, and sulfuric acid, and the current density is 0.1-2.0 mA / cm 2 , the electrolysis time is 30 to 120 seconds; and / or, The conditions of the liquid phase oxidation are: the liquid phase medium is selected from at least one solution of nitric acid, acidic potassium dichromate, sodium hypochlorite, hydrogen peroxide, and potassium persulfate, the concentration of the liquid phase medium is 0.5-5 mol / L, the temperature is 30-80° C., and the time is 1-3 hours; and / or, The gas phase oxidation conditions are: in a mixed atmosphere of air and ozone, the treatment temperature is 150-450° C., and the treatment time is 60-240 seconds; preferably, in the mixed atmosphere, the volume percentage concentration of ozone is 0.5-5.0%.
7. The preparation method according to claim 3, characterized in that: In the step (3): The mass percentage concentration of the sizing agent in the sizing agent solution is 0.5 to 10%, preferably 1 to 5%; and / or, The drying condition is 80-150° C. for 0.5-3 h, preferably 100-120° C. for 1-2 h.
8. A modified chopped carbon fiber prepared by the preparation method according to any one of claims 1 to 7.
9. The modified chopped carbon fiber according to claim 8, characterized in that: The modified chopped carbon fiber comprises carbon fiber and a bundling agent on the surface of the carbon fiber.
10. The modified chopped carbon fiber according to claim 8 or 9, characterized in that: The total fineness of the modified chopped carbon fiber is 3000 to 36000 dtex, preferably 10000 to 30000 dtex; and / or, The aspect ratio of the modified chopped carbon fiber is 500 to 6000, preferably 1000 to 3000; and / or, The surface carbon content of the modified chopped carbon fibers is 50 to 95%, preferably 60 to 80%; and / or, The surface energy of the modified chopped carbon fiber is 50 to 110 mJ / m 2 , preferably 80 to 100 mJ / m 2 and / or, The modified chopped carbon fiber has a dispersion time in water of 5 to 15 seconds; and / or, Based on the total mass of the modified chopped carbon fibers as 100%, the content of the sizing agent on the surface of the carbon fibers is 0.1 to 5%, preferably 0.5 to 3%.
11. Use of the modified chopped carbon fiber according to any one of claims 8 to 10 in a gas diffusion layer of a proton exchange membrane fuel cell.