Waterproof structure of bottom plate

By distributing crystalline waterproof materials into the concrete base plate to form a spatial mesh structure, the poor toughness and hole problems of traditional waterproof materials are solved, the waterproof performance and mechanical strength of concrete are improved, and the service life of concrete is extended.

CN118997232APending Publication Date: 2024-11-22广东建科创新技术研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106381.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

After the existing building waterproofing materials add waterproof coating to the concrete surface, the concrete pores are blocked and the moisture cannot be effectively discharged, resulting in coating damage. In addition, traditional cement-based permeable crystalline waterproofing materials have poor toughness and mismatched expansion coefficients, which are prone to cracking and holes. , reduce the waterproof performance of concrete.

Method used

The concrete bottom layer is composed of a surface layer, a concrete bottom plate and a structural layer. The crystalline waterproof material is evenly distributed in the concrete bottom plate to form a stable spatial network structure, blocking the liquid water and water vapor in the base layer, and passing through lithium silicate and sodium hydroxide The additives react with calcium hydroxide inside the concrete to form C-S-H gel, enhancing density and waterproofing properties.

Benefits of technology

It effectively improves the waterproof performance and mechanical strength of concrete, extends the service life of concrete, and repairs the surface and deep cracks of concrete through the use of reaction accelerators and film-forming agents, and enhances the surface acid, alkali and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118997232A_ABST
    Figure CN118997232A_ABST
Patent Text Reader

Abstract

The invention discloses a bottom plate waterproof structure, which belongs to the field of building waterproof systems and sequentially comprises a surface layer, a concrete bottom plate and a structural layer, and one side, far away from the concrete bottom plate, of the structural layer is in contact with a foundation layer; a capillary crystalline waterproof material is distributed in the concrete bottom plate; the capillary crystalline waterproof material is at least prepared from the following raw materials in percentage by mass: 55.2%-75.1% of lithium silicate, 2.0%-3.6% of sodium hydroxide, 0.8%-1.6% of potassium hydroxide, 0.8%-1.6% of a reaction accelerator, 0.1%-0.15% of a surfactant, 0.3%-0.6% of a film-forming agent, 0.4%-0.8% of anti-crack fibers and the balance of deionized water. A stable space net-shaped structure is constructed in the concrete bottom plate through the capillary crystalline waterproof material, liquid water and water vapor in a foundation layer can be effectively prevented from reaching a surface layer through the concrete bottom plate, and therefore the good protection effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building waterproof systems, and in particular to a baseboard waterproof structure. Background Art

[0002] Modern buildings mostly use reinforced concrete structures as their main body. Under the combined influence of the physical, chemical and biological effects of the surrounding environment, concrete is prone to freeze-thaw, carbonization, alkali-aggregate reaction, cracks, etc., which causes the performance of concrete to decline, and problems such as concrete honeycombs, water leakage, and steel corrosion occur. In terms of the deterioration process, all forms of concrete damage are related to water, and water is also a carrier for the migration of corrosive salts such as chlorides and sulfates. Therefore, how to do a good job of waterproofing concrete has become a key factor in ensuring the long-term durability of concrete.

[0003] The existing waterproofing method is usually to add one or more layers of waterproof coatings such as epoxy resin and polyurethane on the surface of concrete. The waterproofing principle of these waterproof materials is to prevent external moisture from invading the concrete by filling the holes in the concrete. However, since these small holes are blocked, the wall is airtight. Therefore, when moisture is discharged from the pores of the concrete, it will break through the waterproof coating and cause the coating to be damaged. Therefore, the most fundamental solution is to use waterproof materials that reduce the porosity of concrete to increase the rigidity of the concrete itself.

[0004] The commonly used rigid waterproof material is cement-based penetrating crystalline waterproof material. Traditional cement-based penetrating crystalline waterproof materials have defects such as poor toughness, low expansion coefficient matching with cement concrete matrix, and poor interface compatibility, which induce cracks and holes in the waterproof material during service, thereby deteriorating the surface strength and anti-penetration performance of cement concrete, and ultimately leading to premature failure of cement concrete protection and shortening the service life cycle of cement concrete.

[0005] In addition, the existing waterproof structure is usually to coat one side of the concrete layer with one or more layers of waterproof coatings such as epoxy resin and polyurethane. This waterproof structure has many shortcomings. For example, due to the long-term exposure of traditional waterproof materials to the natural environment, they will age, fade and peel off, resulting in the deterioration of the waterproof ability of the concrete layer, causing the concrete to be eroded by water vapor and cause problems such as cracking, corrosion, and water seepage.

[0006] In view of this, the inventor conducted in-depth research on this demand, and thus the present case was produced. Summary of the invention

[0007] Aiming at the problem that the waterproof performance of the base plate waterproof structure of the underground building in the prior art is insufficient, the present invention provides a base plate waterproof structure, which comprises a surface layer, a concrete base plate and a structural layer in sequence, wherein the structural layer is in contact with the base layer at a side away from the concrete base plate;

[0008] The concrete slab is evenly distributed with permeable crystalline waterproof material;

[0009] The penetrating crystallization waterproof material is prepared from at least the following raw materials in percentage by mass: 55.2% to 75.1% lithium silicate, 2.0% to 3.6% sodium hydroxide, 0.8% to 1.6% potassium hydroxide, 0.8% to 1.6% reaction accelerator, 0.1% to 0.15% surfactant, 0.3% to 0.6% film former, 0.4% to 0.8% anti-cracking fiber, and the rest is deionized water.

[0010] The base slab waterproof structure is composed of a surface layer, a concrete base slab and a structural layer, and a penetrating crystalline waterproof material is added to the concrete base slab. A stable spatial network structure is constructed in the concrete base slab using the penetrating crystalline waterproof material, which can effectively block the liquid water and water vapor in the foundation from reaching the surface layer through the concrete base slab, thereby playing a good protective role.

[0011] Preferably, the reaction accelerator is one or both of sodium citrate and sodium aminotriacetate; the film former is one or both of sodium methyl silicate and potassium methyl silicate; the surfactant is one or both of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium chloride.

[0012] Preferably, a permeable crystalline waterproof material is distributed inside the concrete base plate, and the permeable crystalline waterproof material accounts for 0.05-0.10% of the mass of cement in the concrete base plate.

[0013] Preferably, the concrete base plate is prepared from at least the following raw material components, by mass: 300-350 parts of cement, 150-200 parts of water, 620-700 parts of sand, and 1100-1300 parts of crushed stone with a size of 5.0-31.5 mm.

[0014] Preferably, one side of the concrete floor is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0015] Preferably, a polymer self-adhesive film pre-laid waterproofing roll is laid between the concrete base plate and the structural layer, and its thickness is 1.2-10.0 mm. The polymer self-adhesive film pre-laid waterproofing roll is one of the commonly used roll materials for underground buildings. It belongs to plastic waterproofing roll and has no other special requirements. It will not be repeated here. The polymer self-adhesive film pre-laid waterproofing roll, together with the concrete base plate, can not only play a combined waterproofing role, but also effectively improve the lateral strength of the waterproof structure.

[0016] Preferably, C30 fine stone concrete is provided between the surface layer and the concrete base plate, and the thickness of the C30 fine stone concrete is 30-50 mm.

[0017] Preferably, the C30 fine stone concrete is mixed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material accounts for 0.05-0.10% of the cement mass in the fine stone concrete. The C30 fine stone concrete is provided with the permeable crystallization waterproof material added thereto, which, together with the concrete base plate, can play a gradient waterproofing role and also improve the overall strength of the waterproof structure.

[0018] Preferably, the structural layer is a C20 plain concrete cushion layer, and the thickness of the C20 plain concrete cushion layer is 100-300 mm; the side of the concrete bottom plate close to the structural layer is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0019] Preferably, the structural layer is a waterproof coating, waterproof slurry or waterproof membrane with a thickness of 1.2-2.0 mm; the side of the concrete base plate away from the structural layer is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0020] Preferably, the solid content of lithium silicate is 20% to 22%, the modulus is 4.7 to 4.9, and the viscosity of lithium silicate is less than or equal to 25 Pa.s at 25°C.

[0021] Preferably, the effective substance content of sodium hydroxide is greater than 99%.

[0022] Preferably, the effective substance content of potassium hydroxide is greater than 90%.

[0023] Preferably, the anti-cracking fibers are nanocellulose fibrils, and the effective substance content of the anti-cracking fibers is greater than 99%.

[0024] Beneficial effects:

[0025] The beneficial effects produced by the technical solution of the present invention are as follows:

[0026] (1) The base slab waterproof structure is composed of a surface layer, a concrete base slab and a structural layer, and a permeable crystalline waterproof material is added to the concrete base slab. The permeable crystalline waterproof material is used to construct a stable spatial network structure inside the concrete base slab, which can effectively prevent liquid water and water vapor in the base layer from passing through the concrete base slab to reach the surface layer, thereby playing a good protective role.

[0027] (2) Add penetrating crystalline waterproof materials to the concrete base plate. Lithium silicate with a smaller lithium ion radius is mixed with additives such as sodium hydroxide and potassium hydroxide to react chemically with calcium hydroxide in the concrete structure to generate CSH gel. The dendrite-like CSH gel overlaps each other to form a spatial network structure, which can increase the density of the concrete and form an integral waterproof material, thereby improving the mechanical strength of the concrete structure and extending the service life of the concrete.

[0028] (3) The reaction rate of lithium silicate and calcium ions can be effectively controlled by using a reaction accelerator, thereby ensuring that the waterproof material can penetrate deep into the concrete, not only repairing the concrete surface, but also repairing cracks in the concrete from deep inside; the film-forming agent can react chemically with carbon dioxide in the air to form a chemical film, making the concrete surface resistant to acid, alkali and dirt. In addition, this film can prevent surface weathering and improve surface strength, hardness and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is a schematic diagram of the layer structure of the waterproof structure of the bottom plate of the present invention;

[0031] Figure 2 It is a schematic diagram of the layer structure of the second waterproof structure of the bottom plate of the present invention;

[0032] Figure 3 It is a schematic diagram of the layer structure of the bottom plate waterproof structure three of the present invention;

[0033] Figure 4 Schematic diagram of the layer structure of the bottom plate waterproof structure 4 of the present invention;

[0034] Figure 5 It is a schematic diagram of the layer structure of the bottom plate waterproof structure 5 of the present invention.

[0035] In the figure, 1. Surface layer; 2. Concrete base plate; 3. C20 plain concrete cushion layer; 4. Waterproof material layer; 5. Polymer self-adhesive membrane pre-laid waterproofing membrane; 6. Structural layer; 7. C30 fine stone concrete. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] This embodiment adopts the surface layer 1, the concrete bottom plate 2 and the structural layer 6 to form the bottom plate waterproof structure, and the permeable crystallization waterproof material is added into the concrete bottom plate 2, and the permeable crystallization waterproof material is used to construct a stable spatial mesh structure in the concrete bottom plate 2, which can effectively prevent the liquid water and water vapor in the base from passing through the concrete bottom plate 2 to reach the surface layer 1, thereby playing a good protective role. The specific implementation is as follows:

[0038] A base plate waterproof structure, comprising a surface layer 1, a concrete base plate 2 and a structural layer 6 in sequence, wherein the structural layer 6 is in contact with a base layer at a side away from the concrete base plate 2;

[0039] The concrete base plate 2 is provided with permeable crystalline waterproof material;

[0040] The penetrating crystallization waterproof material is prepared from at least the following raw materials in percentage by mass: 55.2% to 75.1% lithium silicate, 2.0% to 3.6% sodium hydroxide, 0.8% to 1.6% potassium hydroxide, 0.8% to 1.6% reaction accelerator, 0.1% to 0.15% surfactant, 0.3% to 0.6% film former, 0.4% to 0.8% anti-cracking fiber, and the rest is deionized water.

[0041] As a preferred embodiment, the reaction accelerator is one or both of sodium citrate and sodium aminotriacetate; the film-forming agent is one or both of sodium methyl silicate and potassium methyl silicate; the surfactant is one or both of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium chloride.

[0042] As a preferred embodiment, a permeable crystallization waterproof material is distributed inside the concrete base plate 2 , and the permeable crystallization waterproof material accounts for 0.05 to 0.10% of the mass of cement in the concrete base plate 2 .

[0043] As a preferred embodiment, the concrete base plate 2 is prepared from at least the following raw material components by mass: 300-350 parts of cement, 150-200 parts of water, 620-700 parts of sand, and 1100-1300 parts of crushed stone with a size of 5.0-31.5 mm.

[0044] As a preferred embodiment, one side of the concrete base plate 2 is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0045] As a preferred embodiment, a polymer self-adhesive film pre-laid waterproofing coiled material 5 is laid between the concrete bottom plate 2 and the structural layer 6, and its thickness is 1.2-10.0 mm. The polymer self-adhesive film pre-laid waterproofing coiled material 5 is one of the coiled material varieties commonly used in underground buildings. It belongs to plastic waterproofing coiled material, and there are no other special requirements for it, which will not be repeated here. The polymer self-adhesive film pre-laid waterproofing coiled material 5, together with the concrete bottom plate 2, can not only play a combined waterproofing role, but also effectively improve the lateral strength of the waterproof structure.

[0046] As a preferred embodiment, C30 fine stone concrete 7 is arranged between the surface layer 1 and the concrete base plate 2, and the thickness of the C30 fine stone concrete 7 is 30-50 mm.

[0047] As a preferred embodiment, the C30 fine stone concrete 7 is mixed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material is 0.05-0.10% of the cement mass in the fine stone concrete. The C30 fine stone concrete 7 is provided with the permeable crystallization waterproof material added thereto, which, together with the concrete bottom plate 2, plays a gradient waterproofing role and can also improve the overall strength of the waterproof structure.

[0048] As a preferred embodiment, the structural layer 6 is a C20 plain concrete cushion layer 3, and the thickness of the C20 plain concrete cushion layer 3 is 100-300 mm; the side of the concrete bottom plate 2 close to the structural layer 6 is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0049] As a preferred embodiment, the structural layer 6 is a waterproof coating, waterproof slurry or waterproof coiled material with a thickness of 1.2-2.0 mm; the side of the concrete base plate 2 away from the structural layer 6 is coated with a permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

[0050] As a preferred embodiment, the solid content of the lithium silicate is 20% to 22%, the modulus is 4.7 to 4.9, and the viscosity of the lithium silicate is less than or equal to 25 Pa.s at 25°C.

[0051] As a preferred embodiment, the effective substance content of the sodium hydroxide is greater than 99%.

[0052] As a preferred embodiment, the effective substance content of the potassium hydroxide is greater than 90%.

[0053] As a preferred embodiment, the anti-cracking fibers are nanocellulose fibrils, and the effective substance content of the anti-cracking fibers is 99.5%.

[0054] This embodiment also provides a method for preparing the above-mentioned permeable crystallization waterproof material, comprising the following steps:

[0055] Step 1, weighing the required mass of lithium silicate, sodium hydroxide, potassium hydroxide and deionized water, and adding them into the reactor in sequence at intervals under a stirring speed of 120 to 150 r / min, with an addition interval of 5 to 10 minutes, stirring for 15 to 30 minutes after the addition is completed, and placing at room temperature to cool to obtain a first mixed solution after the stirring is completed;

[0056] Step 2: laying a microporous filter membrane with a pore size of less than or equal to 0.22 μm in a sand core funnel, then adding 0.1-0.5% of nanocellulose fibrils into the sand core funnel to extract a nanocellulose fibril wet film with a thickness of 0.1-5 mm, adding the extracted nanocellulose fibril wet film to the first mixed solution obtained in step 1 under a stirring speed of 120-150 r / min and stirring for 60-90 minutes, and after the stirring is completed, placing it at room temperature to cool to obtain a second mixed solution;

[0057] Step 3, weighing the required mass of the reaction accelerator and the surfactant, and adding them to the reactor in sequence at intervals under a stirring speed of 120 to 150 r / min, with an addition interval of 5 to 10 min, stirring for 15 to 30 min after the addition is completed, and placing at room temperature to cool to obtain a third mixed solution after the stirring is completed;

[0058] Step 4, adding the second mixed solution and the third mixed solution into a reaction kettle under a stirring speed of 120 to 150 r / min, and stirring for 15 to 30 minutes. After the stirring is completed, the mixture is placed at room temperature to cool to obtain a fourth mixed solution;

[0059] Step 5: adding the film-forming agent to the fourth mixed solution at a stirring speed of 120 to 150 r / min, and stirring for 15 to 30 minutes. After the stirring is completed, the mixture is placed at room temperature to cool to obtain an inorganic aqueous penetrating crystalline waterproofing agent.

[0060] As a preferred embodiment, the bottom plate waterproof structure provided by the present invention is as follows:

[0061] A waterproof structure of the bottom plate, such as Figure 1 As shown, it includes a surface layer 1, a concrete bottom plate 2 and a structural layer 6 in sequence. The structural layer 6 is in contact with the base layer at a side away from the concrete bottom plate 2. The concrete bottom plate 2 is internally provided with a permeable crystalline waterproof material.

[0062] Preferably, the structural layer 6 is a C20 plain concrete cushion, a waterproof coating, a waterproof slurry or a waterproof membrane.

[0063] A waterproof structure of the bottom plate, such as Figure 2 As shown, it includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence; the C20 plain concrete cushion layer 3 is in contact with the base layer at a side away from the concrete base plate 2, and a permeable crystallization waterproof material is distributed inside the concrete base plate 2. The side of the concrete base plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4.

[0064] A waterproof structure of the bottom plate, such as Figure 3 As shown, it includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof membrane 5 and a C20 plain concrete cushion layer 3 in sequence; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and a permeable crystalline waterproof material is distributed inside the concrete base plate 2.

[0065] A waterproof structure of the bottom plate, such as Figure 4 As shown, it includes a surface layer 1, a concrete bottom plate 2 and a structural layer 6 in sequence, wherein the structural layer 6 is in contact with the base layer at a side away from the concrete bottom plate 2, wherein the structural layer 6 is selected from waterproof coating, waterproof slurry or waterproof membrane; a permeable crystallization waterproof material is distributed inside the concrete bottom plate 2. The side of the concrete bottom plate 2 away from the structural layer 6 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4.

[0066] Preferably, the structural layer 6 is selected from SJ polymer cement waterproof coating, polymer cement waterproof slurry (flexible type) or pre-laid reverse-adhesive waterproof membrane.

[0067] A waterproof structure of the bottom plate, such as Figure 5 As shown, it includes a surface layer 1, C30 fine stone concrete 7, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence; the C20 plain concrete cushion layer 3 is in contact with the base layer at the side away from the concrete base plate 2, and a permeable crystalline waterproof material is distributed inside the concrete base plate 2.

[0068] Preferably, the C30 fine stone concrete 7 is mixed with a permeable crystallization waterproof material.

[0069] The beneficial effects of the permeable crystallization waterproof material in this embodiment are further reviewed below through several groups of examples and comparative examples.

[0070] Embodiment 1:

[0071] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0072] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0073] In this embodiment, the bottom plate waterproof structure is as follows:

[0074] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0075] Embodiment 2:

[0076] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0077] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0078] In this embodiment, the bottom plate waterproof structure is as follows:

[0079] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete bottom plate 2. The inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, which is 0.05% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.1 kg / m 2 , the coating thickness is 0.05mm.

[0080] Embodiment 3:

[0081] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0082] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.6%, sodium dodecylbenzene sulfonate 0.15%, potassium methyl silicate 0.6%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0083] In this embodiment, the bottom plate waterproof structure is as follows:

[0084] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof roll 5 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.10% of the mass of cement in the concrete base plate 2.

[0085] Embodiment 4:

[0086] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0087] Lithium silicate 65%, sodium hydroxide 3.0% (effective substance content 99.5%), potassium hydroxide 1.5% (effective substance content 95%), sodium citrate 1.5%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0088] In this embodiment, the bottom plate waterproof structure is as follows:

[0089] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a structural layer 6 in sequence. The structural layer 6 is in contact with the base layer on the side away from the concrete bottom plate 2, wherein the structural layer 6 is a 1.2mm thick pre-laid reverse adhesive waterproofing membrane; the inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material is 0.08% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 away from the structural layer 6 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.2kg / m 2 , the coating thickness is 0.5mm.

[0090] Embodiment 5:

[0091] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0092] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.0%, sodium dodecylbenzene sulfonate 0.13%, potassium methyl silicate 0.4%, nanocellulose fibrils 0.6% (effective substance content 99.5%), and the rest is deionized water.

[0093] In this embodiment, the bottom plate waterproof structure is as follows:

[0094] The base plate waterproof structure includes a surface layer 1, C30 fine stone concrete 7, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the inside of the concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.10% of the mass of cement in the concrete base plate 2.

[0095] The thickness of C30 fine stone concrete 7 is 50 mm, and a permeable crystallization waterproof material is added therein, and the permeable crystallization waterproof material accounts for 0.10% of the mass of cement in the fine stone concrete.

[0096] Embodiment 6:

[0097] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0098] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0099] In this embodiment, the bottom plate waterproof structure is as follows:

[0100] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete bottom plate 2. The inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, which is 0.05% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.15 kg / m 2 , the coating thickness is 0.3mm.

[0101] Embodiment 7:

[0102] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0103] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0104] In this embodiment, the bottom plate waterproof structure is as follows:

[0105] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete bottom plate 2. The inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, which is 0.05% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.2 kg / m 2 , the coating thickness is 0.5mm.

[0106] Embodiment 8:

[0107] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0108] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.6%, sodium dodecylbenzene sulfonate 0.15%, potassium methyl silicate 0.6%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0109] In this embodiment, the bottom plate waterproof structure is as follows:

[0110] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof roll 5 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the concrete base plate 2 is evenly distributed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0111] Embodiment 9:

[0112] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0113] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.6%, sodium dodecylbenzene sulfonate 0.15%, potassium methyl silicate 0.6%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0114] In this embodiment, the bottom plate waterproof structure is as follows:

[0115] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof roll 5 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the concrete base plate 2 is evenly distributed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material is 0.08% of the mass of cement in the concrete base plate 2.

[0116] Embodiment 10:

[0117] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0118] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0119] In this embodiment, the bottom plate waterproof structure is as follows:

[0120] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete bottom plate 2. The inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, which is 0.05% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.08 kg / m 2 , the coating thickness is 0.04mm.

[0121] Embodiment 11:

[0122] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0123] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.6%, sodium dodecylbenzene sulfonate 0.15%, potassium methyl silicate 0.6%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0124] In this embodiment, the bottom plate waterproof structure is as follows:

[0125] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof roll 5 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the concrete base plate 2 is evenly distributed with a penetrating crystalline waterproof material, and the penetrating crystalline waterproof material is 0.04% of the mass of cement in the concrete base plate 2.

[0126] Embodiment 12:

[0127] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0128] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0129] In this embodiment, the bottom plate waterproof structure is as follows:

[0130] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete bottom plate 2. The inside of the concrete bottom plate 2 is evenly distributed with a permeable crystallization waterproof material, which is 0.05% of the cement mass in the concrete bottom plate 2. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.21 kg / m 2 , the coating thickness is 0.53mm.

[0131] Embodiment 13:

[0132] The inorganic water-based permeable crystalline waterproof material in this embodiment is made of the following raw materials by mass percentage:

[0133] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.6%, sodium dodecylbenzene sulfonate 0.15%, potassium methyl silicate 0.6%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0134] In this embodiment, the bottom plate waterproof structure is as follows:

[0135] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2, a polymer self-adhesive membrane pre-laid waterproof roll 5 and a C20 plain concrete cushion layer 3 in sequence, and the thickness of the C20 plain concrete cushion layer 3 is 300 mm; the C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2, and the concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.12% of the mass of cement in the concrete base plate 2.

[0136] Comparative Example 1:

[0137] In this comparative example, the bottom plate waterproof structure does not use inorganic water-based penetrating crystalline waterproof material.

[0138] The waterproof structure of the bottom plate in this comparative example is:

[0139] The base slab waterproof structure includes a surface layer 1, a concrete base slab 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the foundation layer at a side away from the concrete base slab 2.

[0140] Comparative Example 2

[0141] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0142] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0143] The waterproof structure of the bottom plate in this comparative example is:

[0144] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The side of the C20 plain concrete cushion layer 3 away from the concrete bottom plate 2 is in contact with the base layer. The side of the concrete bottom plate 2 close to the C20 plain concrete cushion layer 3 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.1 kg / m 2 , the coating thickness is 0.05mm.

[0145] Comparative Example 3:

[0146] In this comparative example, the bottom plate waterproof structure does not use inorganic water-based penetrating crystalline waterproof material.

[0147] The waterproof structure of the bottom plate in this comparative example is:

[0148] The base slab waterproof structure includes a surface layer 1, a concrete base slab 2, a polymer self-adhesive membrane pre-laid waterproofing membrane 5 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the foundation layer on the side away from the concrete base slab 2.

[0149] Comparative Example 4:

[0150] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0151] Lithium silicate 65%, sodium hydroxide 3.0% (effective substance content 99.5%), potassium hydroxide 1.5% (effective substance content 95%), sodium citrate 1.5%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.8% (effective substance content 99.5%), and the rest is deionized water.

[0152] The waterproof structure of the bottom plate in this comparative example is:

[0153] The bottom plate waterproof structure includes a surface layer 1, a concrete bottom plate 2 and a structural layer 6 in sequence. The structural layer 6 is in contact with the base layer on the side away from the concrete bottom plate 2, wherein the structural layer 6 is a 1.2mm thick pre-laid reverse adhesive waterproofing membrane. The side of the concrete bottom plate 2 away from the structural layer 6 is coated with a permeable crystallization waterproof material to form a waterproof material layer 4, and the coating amount is 0.2kg / m2 , the coating thickness is 0.5mm.

[0154] Comparative Example 5:

[0155] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0156] Lithium silicate 75%, sodium hydroxide 3.6% (effective substance content 99.5%), potassium hydroxide 1.6% (effective substance content 95%), sodium citrate 1.0%, sodium dodecylbenzene sulfonate 0.13%, potassium methyl silicate 0.4%, nanocellulose fibrils 0.6% (effective substance content 99.5%), and the rest is deionized water.

[0157] The waterproof structure of the bottom plate in this comparative example is:

[0158] The base slab waterproof structure includes a surface layer 1, C30 fine stone concrete 7, a concrete base slab 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the foundation layer at the side away from the concrete base slab 2.

[0159] The thickness of C30 fine stone concrete 7 is 50 mm, and a permeable crystallization waterproof material is added therein, and the permeable crystallization waterproof material accounts for 0.10% of the mass of cement in the fine stone concrete.

[0160] Comparative Example 6:

[0161] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0162] Lithium silicate 54%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0163] The waterproof structure of the bottom plate in this comparative example is:

[0164] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0165] Comparative Example 7:

[0166] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0167] Lithium silicate 56%, sodium hydroxide 1.8% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0168] The waterproof structure of the bottom plate in this comparative example is:

[0169] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0170] Comparative Example 8:

[0171] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0172] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.6% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0173] The waterproof structure of the bottom plate in this comparative example is:

[0174] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0175] Comparative Example 9:

[0176] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0177] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.6%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0178] The waterproof structure of the bottom plate in this comparative example is:

[0179] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0180] Comparative Example 10:

[0181] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0182] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.08%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0183] The waterproof structure of the bottom plate in this comparative example is:

[0184] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0185] Comparative Example 11:

[0186] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0187] Lithium silicate 77%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0188] The waterproof structure of the bottom plate in this comparative example is:

[0189] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0190] Comparative Example 12:

[0191] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0192] Lithium silicate 56%, sodium hydroxide 3.8% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0193] The waterproof structure of the bottom plate in this comparative example is:

[0194] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0195] Comparative Example 13:

[0196] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0197] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 1.9% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0198] The waterproof structure of the bottom plate in this comparative example is:

[0199] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0200] Comparative Example 14:

[0201] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0202] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 1.8%, sodium dodecylbenzene sulfonate 0.10%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0203] The waterproof structure of the bottom plate in this comparative example is:

[0204] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0205] Comparative Example 15:

[0206] The inorganic water-based permeable crystalline waterproof material in this comparative example is made of the following raw materials by mass percentage:

[0207] Lithium silicate 56%, sodium hydroxide 2.0% (effective substance content 99.5%), potassium hydroxide 0.8% (effective substance content 95%), sodium citrate 0.8%, sodium dodecylbenzene sulfonate 0.19%, potassium methyl silicate 0.3%, nanocellulose fibrils 0.4% (effective substance content 99.5%), and the rest is deionized water.

[0208] The waterproof structure of the bottom plate in this comparative example is:

[0209] The base plate waterproof structure includes a surface layer 1, a concrete base plate 2 and a C20 plain concrete cushion layer 3 in sequence. The thickness of the C20 plain concrete cushion layer 3 is 300 mm. The C20 plain concrete cushion layer 3 is in contact with the base layer on the side away from the concrete base plate 2. The concrete base plate 2 is evenly distributed with a permeable crystalline waterproof material, and the permeable crystalline waterproof material is 0.05% of the mass of cement in the concrete base plate 2.

[0210] The preparation method of the inorganic water-based permeable crystalline waterproof material in the above-mentioned implementation and comparative examples comprises the following steps:

[0211] Step 1, weighing the required mass of lithium silicate, sodium hydroxide, potassium hydroxide and deionized water, and adding them into the reactor in sequence at intervals under a stirring environment with a stirring speed of 120r / min, with an addition interval of 10min, stirring for 20min after the addition is completed, and leaving it to cool at room temperature after the stirring is completed to obtain a first mixed solution;

[0212] Step 2: Lay a microporous filter membrane with a pore size of 0.18 μm in a sand core funnel with a diameter of 7.4 cm, then stir 0.2% of nanocellulose fibrils and add them into the sand core funnel to extract a nanocellulose fibril wet film with a thickness of 0.3 mm, add the extracted nanocellulose fibril wet film to the first mixed solution obtained in step 1 under a stirring speed of 120 r / min and stir for 60 minutes, and after the stirring is completed, place it at room temperature to cool to obtain a second mixed solution;

[0213] Step 3, weighing the required mass of the reaction accelerator and the surfactant, and adding them to the reactor in sequence at intervals under a stirring speed of 120 r / min, with an addition interval of 5 min, stirring for 15 min after the addition, and leaving to cool at room temperature to obtain a third mixed solution;

[0214] Step 4, adding the second mixed solution and the third mixed solution into a reaction kettle under a stirring condition at a stirring speed of 120 r / min, and stirring for 15 minutes. After the stirring is completed, the mixture is placed under room temperature to cool to obtain a fourth mixed solution;

[0215] Step 5: adding the film-forming agent into the fourth mixed solution at a stirring speed of 120 r / min, and stirring for 15 minutes. After the stirring is completed, the mixture is placed at room temperature to cool to obtain a permeable crystalline waterproof material.

[0216] Table 1 Concrete mix ratio for each group

[0217]

[0218] A concrete base plate is selected, and the proportion of each component thereof is shown in Table 1. The waterproof material is mixed and stirred with the components in the concrete as described in the embodiments and comparative examples, and the concrete base plate is obtained after molding. After the concrete base plate is formed, it is cured under standard conditions for 28 days, and then a waterproof base plate structure is formed with other structures as described in the embodiments and comparative examples. Finally, the waterproof base plate structure obtained in the embodiments and comparative examples is subjected to performance tests according to the "Test Method for Long-term Performance and Durability of Ordinary Concrete" (GB / T50082-2009), and the performance indicators are shown in Table 2.

[0219] Table 2 Waterproof performance test results

[0220]

[0221]

[0222]

[0223] It can be seen from the test results of Examples 1 to 9 in Table 2 that the use of waterproof materials within any given component content range in combination with any baseboard waterproof structure provided in the present application has a good waterproof effect, and the 48h water absorption ratio of the baseboard waterproof structure is significantly reduced.

[0224] Comparing the test results of Examples 2 and 3 with those of Examples 10 and 11, it can be seen that when the amount of waterproof material added to the concrete base plate, the amount of coating on the surface of the concrete base plate and the coating thickness are lower than the usage amount given in this application, the waterproof ability of the base plate waterproof structure using the waterproof material will be slightly reduced; and comparing the test results of Examples 2 and 3 with those of Examples 12 and 13, as the usage amount of the waterproof material increases and exceeds the range given in this application, the waterproof ability of the waterproof base plate structure is not significantly improved. Therefore, out of consideration of the balance between waterproof effect and use cost, the usage range of the waterproof material given in this application is a better choice.

[0225] By comparing the test results of Examples 1 to 5 with those of Comparative Examples 1 to 5, it can be seen that the waterproof material with a component content within a given range mixed into the concrete base plate can greatly improve the waterproof base plate's anti-seepage grade and significantly reduce the water absorption, indicating that the water-based permeable crystalline waterproof material mixed into the concrete base plate has a good protective effect on the concrete and can significantly improve the concrete's anti-seepage grade. It is obvious that the waterproof effect of mixing the waterproof material into the concrete is much better than the waterproof effect of coating the waterproof material on one side of the concrete base plate or adding a waterproof layer. The 48h water absorption of the base plate waterproof structure obtained by mixing the waterproof material into the concrete base plate is significantly reduced, and its anti-seepage grade is at a relatively high level, indicating that mixing the waterproof material into the concrete floor can better exert its waterproof and anti-seepage capabilities.

[0226] Comparing the test results of Example 1 with those of Comparative Examples 6 to 15, the contents of key components in the waterproof material, such as lithium silicate, sodium hydroxide, potassium hydroxide, reaction accelerator and surfactant, which are lower or higher than the content range of each component of the waterproof material given in the present application, will reduce the waterproof and protective effect of the waterproof material on the concrete base plate.

[0227] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A baseboard waterproof structure, characterized in that: It comprises a surface layer, a concrete bottom plate and a structural layer in sequence, wherein the structural layer is in contact with the foundation layer at a side away from the concrete bottom plate; The concrete bottom plate is provided with a permeable crystallized waterproof material; The penetrating crystallization waterproof material is prepared from at least the following raw materials, calculated by mass percentage: 55.2% to 75.1% lithium silicate, 2.0% to 3.6% sodium hydroxide, 0.8% to 1.6% potassium hydroxide, 0.8% to 1.6% reaction accelerator, 0.1% to 0.15% surfactant, 0.3% to 0.6% film former, 0.4% to 0.8% anti-cracking fiber, and the rest is deionized water.

2. A bottom plate waterproof structure according to claim 1, characterized in that: The reaction accelerator is one or both of sodium citrate and sodium aminotriacetate; the film-forming agent is one or both of sodium methyl silicate and potassium methyl silicate; the surfactant is one or both of sodium dodecylbenzene sulfonate and dodecyltrimethylammonium chloride.

3. A bottom plate waterproof structure according to claim 1, characterized in that: The permeable crystallization waterproof material is distributed inside the concrete bottom plate, and the permeable crystallization waterproof material accounts for 0.05-0.10% of the mass of cement in the concrete bottom plate.

4. A bottom plate waterproof structure according to claim 1, characterized in that: The concrete base plate is prepared from at least the following raw material components by weight: 300-350 parts of cement, 150-200 parts of water, 620-700 parts of sand, and 1100-1300 parts of crushed stone with a size of 5.0-31.5 mm.

5. The bottom plate waterproof structure according to claim 1, characterized in that: One side of the concrete bottom plate is coated with the permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.

6. A bottom plate waterproof structure according to claim 1, characterized in that: A polymer self-adhesive pre-laid waterproofing coiled material is laid between the concrete bottom plate and the structural layer, and the thickness of the pre-laid waterproofing coiled material is 1.2-10.0 mm.

7. A bottom plate waterproof structure according to claim 1, characterized in that: C30 fine stone concrete is arranged between the surface layer and the concrete bottom plate, and the thickness of the concrete fine stone concrete is 30-50 mm.

8. A bottom plate waterproof structure according to claim 7, characterized in that: The C30 fine stone concrete is mixed with a permeable crystallization waterproof material, and the permeable crystallization waterproof material accounts for 0.05-0.10% of the mass of cement in the fine stone concrete.

9. The bottom plate waterproof structure according to claim 1, characterized in that: The structural layer is a C20 plain concrete cushion layer, and the thickness of the C20 plain concrete cushion layer is 100-300mm; the side of the concrete bottom plate close to the structural layer is coated with the permeable crystallization waterproof material, and the coating amount is 0.1-0.2kg / m 2 , the coating thickness is 0.05~0.5mm.

10. The bottom plate waterproof structure according to claim 1, characterized in that: The structural layer is a waterproof coating, waterproof slurry or waterproof coiled material with a thickness of 1.2-2.0 mm; the side of the concrete base plate away from the structural layer is coated with the permeable crystallization waterproof material, and the coating amount is 0.1-0.2 kg / m 2 , the coating thickness is 0.05~0.5mm.