Method for measuring true stress and work hardening rate after stretching and necking and application
Through a uniaxial tensile test and a video extensometer, the true stress and true strain after necking of the refractory high-entropy alloy were calculated, and the inaccurate measurement in the prior art was solved. The problem of the problem achieves a more accurate assessment of mechanical behavior.
Patent Information
- Application Number
- CN202411103924.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to accurately measure the true stress and true strain of refractory high-entropy alloys after necking at room temperature, resulting in inaccurate measurement of mechanical behavior, affecting the structural design and forming process development of the material.
The engineering stress-strain curve and true stress-true strain curve were obtained through uniaxial tensile test, and the critical neck strain point was determined. The width change of the neck center section was measured using a video extensometer, and the deformation ratio of thickness and width was calculated. For the true stress and true strain data after shrinkage, draw the true stress-true strain curve and work hardening rate curve after necking.
Provides more accurate mechanical behavior data after necking, ensuring the authenticity and accuracy of the measurement, suitable for measurements of true stress-true strain and work hardening rates throughout the tensile process, helping engineers evaluate material properties and select suitable material.
Smart Images

Figure CN119000238A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material measurement, and in particular to a method and application for measuring true stress and work hardening rate after stretching and necking. Background Art
[0002] Necking is an important failure mechanism that is widely present in various materials, such as metals and concrete. Its main feature is that the strain field changes sharply from a uniform distribution mode to a non-uniform distribution mode. According to the tensile mechanical behavior of materials, materials can be divided into two categories: brittle materials and ductile materials. Brittle materials only undergo elastic deformation before fracture, while ductile materials begin to undergo irreversible plastic deformation after elastic deformation. Plastic deformation can be divided into uniform plastic deformation stage and non-uniform plastic deformation stage. Non-uniform plastic deformation, also known as necking, is the most significant phenomenon of macroscopic strain localization that occurs after the load reaches the peak value. As the simplest and most easily operated means of studying the mechanical properties of materials, the tensile test measures load-displacement curves and stress-strain curves based on the material being in a single-phase stress state, and this ideal state can only last until the end of the uniform plastic deformation stage. When the specimen necks, the elongation is no longer uniformly distributed along the standard specimen distance segment, and is large in the necking zone and small outside the necking zone. Characterizing the material using the change in gauge length has lost its original physical meaning, and the true stress work hardening obtained from it is also inaccurate. Therefore, obtaining accurate mechanical behavior after necking is crucial for engineers to predict the deformation behavior of materials and better select materials for structural design and forming process development.
[0003] High entropy alloys are new alloy materials developed in recent years. Compared with traditional alloys, they have higher strength, wear resistance, corrosion resistance and high hardness, and have broad application prospects. Refractory high entropy alloys are a subclass of high entropy alloys. They have higher high temperature strength than traditional nickel-based alloys, but most refractory high entropy alloys have poor plasticity and toughness at room temperature, which is not conducive to processing and forming. Therefore, special attention is paid to refractory high entropy alloys such as HfNbTaTiZr and TiVNbTa that exhibit tensile plasticity at room temperature. Although they have good tensile plasticity, their processing ability is weak, and they soften after yielding. The elongation is mainly reflected in non-uniform elongation. Therefore, it is very important to understand the mechanical behavior of such alloys after necking. However, the current methods for measuring the true stress strain and work hardening of alloys after necking are not accurate. Summary of the invention
[0004] In order to solve the deficiencies existing in the above-mentioned background technology, mainly aiming at the problems in the prior art that the width of the necking cross-section is difficult to measure and the measurement of the true stress-true strain value after necking is inaccurate, the present invention provides a method for measuring the true stress and work hardening rate after tensile necking and its application. This method only needs to know the width change of the necking center section during the stretching process to obtain the accurate mechanical behavior after necking.
[0005] In order to achieve the above object, the first object of the present invention is to provide a method for measuring true stress and work hardening rate after tensile necking, comprising the following steps: Based on the uniaxial tensile test, the engineering stress-strain curve of the sample is obtained, and the true stress-true strain curve before necking and the work hardening rate curve are obtained; The critical necking strain point is determined according to the intersection of the true stress-true strain curve before necking and the work hardening rate curve; After the sample is stretched to reach the critical necking strain, the width of the sample necking center section is measured based on the tensile video extensometer; Define the deformation of the thickness of the sample's necking center surface to be in a certain ratio to the width deformation, and obtain the cross-sectional area of the sample's necking center; The true stress and true strain data after necking are calculated according to the cross-sectional area of the sample's necking center, and the true stress-true strain curve and work hardening rate curve after necking are plotted; Based on the true stress-true strain curve and work hardening rate curve before necking, as well as the true stress-true strain curve and work hardening rate curve after necking, the true stress-true strain curve and work hardening rate curve of the entire tensile process are obtained.
[0006] Preferably, obtaining the engineering stress-strain curve of the sample includes obtaining the engineering stress and the engineering strain, and drawing the engineering stress-strain curve according to the engineering stress and the engineering strain, wherein the engineering stress calculation formula is as follows:
[0007] The engineering strain calculation formula is as follows:
[0008] In the formula, represents engineering stress; F Indicates the force of the tensile test; represents the initial cross-sectional area; represents engineering strain; Indicates the initial gauge length; Indicates the length of the gauge segment after stretching.
[0009] Preferably, the true stress-true strain curve before necking is drawn based on true stress and true strain, wherein the true stress calculation formula is as follows:
[0010] The true strain calculation formula is as follows:
[0011] In the formula, represents the true stress, Represents true strain. This is the traditional method for calculating true stress and true strain, and is accurate before necking.
[0012] Preferably, the work hardening rate curve is obtained by differentiating a true stress-true strain curve.
[0013] Preferably, the deformation of the thickness of the central surface of the sample necking is in a certain proportion to the deformation of the width, and the calculation formula is as follows:
[0014]
[0015]
[0016] In the formula, represents the shape scale factor, represents the initial thickness of the sample, represents the instantaneous thickness of the sample, represents the change in thickness, represents the initial width of the sample, represents the instantaneous width of the sample, Indicates the change in width.
[0017] Preferably, the true stress-true strain curve after necking is drawn based on the true stress and true strain after necking, wherein the true stress after necking is calculated by the following formula:
[0018] The true strain after necking is calculated as follows:
[0019] In the formula, Local true strain, represents the local true stress, It represents the cross-sectional area of the neck center during stretching; F Indicates the force of the tensile test; represents the initial cross-sectional area.
[0020] Preferably, the work hardening rate curve after necking is obtained by differentiating the true stress-true strain curve after necking.
[0021] Preferably, the cross-sectional area of the sample necking center is obtained according to the following steps: The thickness of the sample is obtained by defining the deformation of the thickness of the sample's necking center surface in a certain ratio to the width deformation; the cross-sectional area of the sample's necking center is calculated based on the width and thickness of the sample.
[0022] Preferably, the true stress and true strain data points after necking are calculated according to the following steps: Obtain the force of the tensile test; According to the applied force of the tensile test and the necking center cross-sectional area and the initial cross-sectional area during stretching, the true stress and true strain data points after necking are obtained.
[0023] The second object of the present invention is to provide an application of the above method in measuring the mechanical behavior of metals or alloys after necking.
[0024] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for measuring true stress, true strain and work hardening rate after stretching and necking, and its application. The traditional method for measuring true stress, strain and work hardening is only applicable to uniform deformation before necking, and is not applicable to measuring non-uniform deformation after necking. The present invention provides more realistic and accurate true stress, true strain and work hardening rate values, thereby obtaining the true stress-true strain curve and work hardening curve of the complete stretching process. The measurement method and calculation adopted by the present invention are relatively simple and have a wide range of applications. Using the present invention, the true stress, true strain and work hardening rate of the material in the complete stretching process can be accurately measured as needed, providing guidance for scientific researchers and engineers to evaluate the deformation behavior of materials, assess the mechanical properties of materials, and better select materials for structural design and forming process development. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention provides a flow chart of a method for measuring true stress and work hardening after necking.
[0026] Figure 2 is the engineering stress-strain curve.
[0027] Figure 3 It is the true stress-true strain curve and work hardening curve.
[0028] Figure 4 This is the deformation morphology of the sample during the tensile process.
[0029] Figure 5 The true stress-true strain curve and the work hardening curve of the as-cast refractory high entropy alloy measured according to the present invention. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0031] The purpose of the present invention is to provide a method and application for measuring the true stress and work hardening rate after tensile necking. The method mainly includes three parts: first, obtaining the uniaxial tensile properties of the material, determining the critical necking strain, then obtaining the minimum cross-sectional area of the necking, and finally calculating the true stress strain and work hardening after necking based on the minimum cross-sectional area.
[0032] In order to achieve the above object, the present invention provides a method for measuring true stress and work hardening rate after stretching and necking, comprising the following steps: S1. Based on the uniaxial tensile test, obtain the engineering stress-strain curve of the sample, and obtain the true stress-true strain curve and work hardening rate curve before necking; Wherein, when obtaining the engineering stress-strain curve of the sample, it includes obtaining the engineering stress and engineering strain, and drawing the engineering stress-strain curve according to the engineering stress and engineering strain, wherein the engineering stress calculation formula is as follows:
[0033] The engineering strain calculation formula is as follows:
[0034] In the formula, represents engineering stress; F Indicates the force of the tensile test; represents the initial cross-sectional area; represents engineering strain; Indicates the initial gauge length; Indicates the length of the gauge segment after stretching.
[0035] The true stress-true strain curve before necking is drawn based on the true stress and true strain, wherein the true stress calculation formula before necking is as follows:
[0036] The true strain calculation formula is as follows:
[0037] In the formula, represents the true stress, Represents true strain. This is the traditional method for calculating true stress and true strain, and is accurate before necking.
[0038] The work hardening rate curve before necking is obtained by differentiating the true stress-true strain curve, and its calculation formula is as follows: .
[0039] The uniaxial stretching is performed at room temperature using a dog-bone-shaped specimen.
[0040] S2. Determine the critical necking strain point according to the intersection of the true stress-true strain curve before necking and the work hardening rate curve; the critical necking strain point is obtained according to the following steps: The dog-bone specimens were subjected to uniaxial tension at room temperature to obtain the engineering stress-strain curve, the true stress-true strain curve and the work hardening rate curve converted from the engineering stress-strain.
[0041] The intersection of the work hardening rate curve and the true stress-true strain curve is taken as the critical necking strain point.
[0042] It should be noted that the true stress-true strain curve and work hardening rate curve obtained by engineering stress-strain conversion can only be retained before the necking strain point. After the necking strain point, due to the local deformation of the specimen, the results calculated by this method are not accurate.
[0043] S3, after the sample is stretched to reach the critical necking strain, the width of the sample necking center section is measured based on the tensile video extensometer; The width of the necked center section is measured by a video extensometer in real time to measure the change of the sample along the width direction.
[0044] S4, defining that the deformation of the thickness of the sample's necking center surface is in a certain ratio to the deformation of the width, and obtaining the cross-sectional area of the sample's necking center; The thickness deformation of the sample necking center plane is defined to be in a certain proportion to the width deformation, and the calculation formula is as follows:
[0045]
[0046]
[0047] In the formula, represents the shape scale factor, represents the initial thickness of the sample, represents the instantaneous thickness of the sample, represents the change in thickness, represents the initial width of the sample, represents the instantaneous width of the sample, Indicates the change in width; the cross-sectional area of the sample necking center, = * .
[0048] S5. Calculate the true stress and true strain data points after necking according to the cross-sectional area of the necking center of the sample, and draw the true stress-true strain curve and work hardening rate curve after necking; The cross-sectional area of the sample necking center is obtained by following the steps below: The thickness of the sample is obtained by defining the deformation of the thickness of the sample's necking center surface in a certain ratio to the width deformation; the cross-sectional area of the sample's necking center is calculated based on the width and thickness of the sample.
[0049] It should be noted that it is assumed based on experience that the deformation of the thickness of the sample's necking center surface is in a certain proportion to the deformation of its width.
[0050] The true stress and true strain data points after necking are calculated according to the following steps: Obtain the force of the tensile test; According to the applied force of the tensile test and the necking center cross-sectional area and the initial cross-sectional area during stretching, the true stress and true strain data points after necking are obtained.
[0051] The true stress-true strain curve after necking is drawn based on the true stress and true strain after necking, wherein the true stress after necking is calculated by the following formula:
[0052] The true strain after necking is calculated as follows:
[0053] In the formula, Local true strain, represents the local true stress, It represents the cross-sectional area of the neck center during stretching; F Indicates the force of the tensile test; represents the initial cross-sectional area.
[0054] The work hardening rate curve after necking is obtained by differentiating the true stress-true strain curve after necking. , is to differentiate the true stress-true strain curve after necking. According to the engineering stress-strain, the true stress-strain and work hardening law before necking are obtained, and according to the width and thickness of the sample necking center plane measured in real time, the true stress and work hardening rate law after necking are obtained. The processing rates before and after necking calculated by these two methods have certain errors at the critical necking strain point, which are connected by dotted lines.
[0055] S6. Based on the true stress-true strain curve and work hardening rate curve before necking, as well as the true stress-true strain curve and work hardening rate curve after necking, the true stress-true strain curve and work hardening rate curve of the entire stretching process are obtained.
[0056] The method of obtaining the true stress-true strain curve and the work hardening rate curve of the entire stretching process includes: According to the engineering stress and strain, the true stress and strain before necking are obtained; According to the real-time measurement of the width and thickness of the sample necking center plane, the true stress and strain after necking are obtained; The true stress-strain data before and after necking are combined and differentiated to obtain the true stress-true strain curve and work hardening rate curve of the entire tensile process.
[0057] The invention also provides an application in measuring the true stress and work hardening rate of the alloy after tensile necking.
[0058] In order to illustrate the method for measuring true stress and work hardening after necking provided by the present invention, it is described in conjunction with the accompanying drawings.
[0059] See also Figure 1 A method for measuring true stress and work hardening after necking is shown, comprising: This embodiment selects the cast HfNbTaTiZr refractory high entropy alloy to measure the true stress and work hardening after necking. First, the cast HfNbTaTiZr refractory high entropy alloy is uniaxially stretched, and then its engineering stress-strain curve, true stress-true strain curve and work hardening rate curve are obtained to determine the critical necking strain point. Then, the change in the width direction during stretching is obtained according to the video extensometer, and it is assumed that the thickness change is in a certain proportion to the width change, so as to calculate the minimum cross-sectional area, and finally the true stress-true strain and work hardening of the HfNbTaTiZr refractory high entropy alloy before and after necking are obtained. The specific steps are as follows: Step 1: Calculate the engineering stress under uniaxial tension using formula (1) and formula (2) ,strain , using formula (3) and formula (4) to obtain the true stress True strain , using formula (5) to get the work hardening rate: (1) (2) (3) (4) (5) In formulas (1), (2), (3), (4) and (5), represents the engineering stress, is the force of the tensile test, represents the initial cross-sectional area, represents the engineering strain, represents the initial gauge length, Indicates the instantaneous gauge length, represents the true stress, The yield strength of HfNbTaTiZr refractory high entropy is 919 MPa, and the ultimate tensile strength is 946 MPa. Figure 2 By plotting the intersection of the work hardening rate curve and the true stress-true strain curve, the critical necking strain is obtained. ,like Figure 3 shown.
[0060] Step 2: Using the video extensometer, measure the change in the width of the necking center section during the stretching process of the sample in real time, and assume that the deformation of the thickness and width of the necking center surface of the sample satisfies the following relationship: (6) (7) (8) In formulas (6), (7) and (8), represents the shape ratio coefficient, when hour, The value is 1, when hour, The value is 0.49. represents the initial thickness of the sample, represents the instantaneous thickness of the sample, represents the change in thickness, represents the initial width of the sample, represents the instantaneous width of the sample, Indicates the change in width. The initial width of the sample is 1800 μm and the thickness is 790 μm. The value is 0.49. The width of the sample changes during the stretching process. Figure 4 shown.
[0061] Step 3: Use formulas (9) and (10) to calculate the true stress and strain after necking: (9) (10) In formulas (9) and (10), Local true strain, Represents the local true stress. Table 1 gives the true stress-true strain values after necking at different times. The stress-strain curve and work hardening rate curve are shown in Figure 5 As shown. The present invention is used to measure the true stress and true strain after necking, and the work hardening rate is still stable within a larger strain range, and the maximum true stress can reach 1495MPa. The local true stress and true strain after necking can be described more accurately.
[0062] Table 1 True stress and true strain after necking
[0063] Compare the true stress-true strain curve and work hardening rate curve calculated by formula (3) and formula (4).
[0064] Figure 5 It is the true stress-true strain curve and work hardening curve calculated by the method of the present invention. The true stress and true strain calculated by the present invention are compared with the true stress-strain calculated by the change of the gauge section length (traditional method). The two methods have the same change trend, but the maximum stress value and the maximum strain value are different. The true stress measured by the present invention can reach up to 1495 MPa. Comparing the work hardening curve calculated by the method of the present invention with the work hardening curve obtained by the traditional method, it can be seen that the work hardening rate measured by the present invention remains unchanged within a larger strain range. The measurement method of the present invention can more accurately describe the true stress, true strain and work hardening rate of local deformation, and the method is simple and the calculation is fast.
[0065] The present invention describes preferred embodiments and their effects. However, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0066] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for measuring true stress and work hardening rate after tensile necking, characterized in that: The following steps are involved: Based on the uniaxial tensile test, the engineering stress-strain curve of the sample is obtained; and the true stress-true strain curve and the work hardening rate curve before necking are obtained; The critical necking strain point is determined according to the intersection of the true stress-true strain curve before necking and the work hardening rate curve; After the sample is stretched to reach the critical necking strain, the width of the sample necking center section is measured based on the tensile video extensometer; Define the deformation of the thickness of the sample's necking center surface to be in a certain ratio to the width deformation, and obtain the cross-sectional area of the sample's necking center; According to the cross-sectional area of the sample's necking center, the true stress and true strain data points after necking are calculated, and the true stress-true strain curve and work hardening rate curve after necking are plotted; Based on the true stress-true strain curve and work hardening rate curve before necking, as well as the true stress-true strain curve and work hardening rate curve after necking, the true stress-true strain curve and work hardening rate curve of the entire stretching process are obtained.
2. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: When obtaining the engineering stress-strain curve of the sample, it includes obtaining the engineering stress and engineering strain, and drawing the engineering stress-strain curve according to the engineering stress and engineering strain, wherein the engineering stress calculation formula is as follows: The engineering strain calculation formula is as follows: In the formula, represents engineering stress; F Indicates the force of the tensile test; represents the initial cross-sectional area; represents engineering strain; Indicates the initial gauge length; Indicates the length of the gauge segment after stretching.
3. The method for measuring true stress and work hardening rate after tensile necking according to claim 2, characterized in that: The true stress-true strain curve before necking is drawn based on the true stress and true strain, wherein the true stress calculation formula is as follows: The true strain calculation formula is as follows: In the formula, represents the true stress, Indicates true strain.
4. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The work hardening rate curve before necking is obtained by differentiating the true stress-true strain curve before necking.
5. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The change in thickness of the sample's necking center plane is defined to be in a certain proportion to the change in width, and the calculation formula is as follows: In the formula, represents the shape scale factor, represents the initial thickness of the sample, represents the instantaneous thickness of the sample, represents the change in thickness, represents the initial width of the sample, represents the instantaneous width of the sample, Indicates the change in width.
6. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The true stress-true strain curve after necking is drawn based on the true stress and true strain after necking, wherein the true stress after necking is calculated by the following formula: The true strain after necking is calculated as follows: In the formula, Local true strain, represents the local true stress, It represents the cross-sectional area of the neck center during stretching; F Indicates the force of the tensile test; represents the initial cross-sectional area.
7. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The work hardening rate curve after necking is obtained by differentiating the true stress-true strain curve after necking.
8. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The cross-sectional area of the sample necking center is obtained by following the steps below: The thickness of the sample is obtained by defining the deformation of the thickness of the sample's necking center surface in a certain ratio to the width deformation; the cross-sectional area of the sample's necking center is calculated based on the width and thickness of the sample.
9. The method for measuring true stress and work hardening rate after tensile necking according to claim 1, characterized in that: The true stress and true strain data points after necking are calculated according to the following steps: Obtain the force of the tensile test; According to the applied force of the tensile test and the necking center cross-sectional area and the initial cross-sectional area during stretching, the true stress and true strain data points after necking are obtained.
10. Use of the method according to any one of claims 1 to 9 in measuring the mechanical behavior of metals or alloys after necking.