Method for testing inherent molecular weight distribution type of raw natural rubber
Through the frequency scanning method of rotor-free shear rheometer, the logarithmic relationship curve between loss modulus and frequency is established, and the inherent molecular weight distribution type of natural rubber raw rubber is accurately distinguished, and the problem that cannot accurately reflect the inherent characteristics in the prior art is solved. , realize effective classification and performance optimization of rubber tree varieties.
Patent Information
- Application Number
- CN202411162419.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing testing methods cannot accurately reflect the inherent molecular weight distribution of natural rubber raw rubber, resulting in the inability to effectively distinguish the inherent characteristics of rubber tree varieties, affecting their processing performance and application performance.
The rotor-free shear rheometer is used for sample adjustment and frequency scanning to establish a logarithmic relationship curve between loss modulus and scanning frequency. The inherent molecular weight distribution type of natural rubber raw rubber is determined through the curve characteristics, and distinguished into single peaks and double peaks. distributed.
It realizes the rapid and accurate identification of the inherent molecular weight distribution type of natural rubber raw rubber, and can trace the "family" information of the rubber tree, avoiding errors caused by gel filtration in traditional methods, and improving the accuracy of the test.
Smart Images

Figure CN119000428A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of natural rubber raw rubber molecular weight distribution, in particular to a method for testing the inherent molecular weight distribution type of natural rubber raw rubber. Background Art
[0002] The superior comprehensive mechanical properties and irreplaceability of natural rubber are derived from its unique molecular structure given by biosynthesis. Among them, bimodal molecular weight distribution is one of the important structural characteristics of natural rubber. In fact, the molecular weight distribution type of natural rubber is related to the genotype of the rubber tree variety, and is also affected by the molecular chain crosslinking (gel formation) and oxidative chain scission (such as high temperature drying) during the preparation of raw rubber from latex and the storage of raw rubber. Excluding the influence of molecular chain crosslinking and oxidative chain scission, the molecular weight distribution that can reflect the inherent characteristics of rubber tree varieties is called inherent molecular weight distribution. According to the different inherent molecular weight distribution types, rubber tree varieties can be divided into "single-peak family" and "bimodal family". A large number of studies have shown that raw rubber prepared from latex produced by rubber tree varieties of "single-peak family" or "bimodal family" has significantly different processing properties and application properties. Among them, natural rubber with bimodal molecular weight distribution can obtain a better straightening force / elongation curve in the unprocessed state, thereby improving the performance of tire products. Therefore, it is very meaningful for product users to master the information on the direction of the molecular weight distribution type of natural rubber raw rubber. During the preparation of raw rubber from latex and the storage of raw rubber, the natural rubber molecular chains will undergo structuring and produce gel. When using traditional methods (such as gel permeation chromatography) to test the molecular weight of natural rubber, the gel in the sample solution must be filtered out first, resulting in the test results not being able to accurately reflect the inherent molecular weight distribution. Summary of the invention
[0003] The object of the present invention is to provide a method for testing the inherent molecular weight distribution type of natural rubber raw rubber. The method can quickly and accurately identify the inherent molecular weight distribution type of natural rubber raw rubber, and realize the traceability of the rubber tree "family" of the latex source used in the raw rubber preparation.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a method for testing the inherent molecular weight distribution type of natural rubber raw rubber, comprising the following steps:
[0006] Using a rotorless shear rheometer, the natural rubber raw rubber was subjected to sample conditioning and frequency scanning in sequence to obtain a series of scanning frequencies and loss moduli;
[0007] With the scanning frequency as the logarithmic abscissa and the loss modulus as the logarithmic ordinate, a logarithmic relationship curve between the loss modulus and the scanning frequency is established;
[0008] The inherent molecular weight distribution type of the natural rubber raw rubber is determined by the relationship curve between the loss modulus and the scanning frequency: when the loss modulus increases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is bimodal; when the loss modulus decreases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is unimodal.
[0009] Preferably, the natural rubber raw rubber is natural rubber raw rubber that has not been roller-refined.
[0010] Preferably, the sample is conditioned for 2 to 8 minutes, at a temperature of 80 to 130° C., at a frequency of 0.1 to 0.5 Hz, and at a strain of 2.8% to 7%.
[0011] Preferably, the sample is conditioned for 3 to 7 minutes, at a temperature of 90 to 120° C., at a frequency of 0.1 to 0.4 Hz, and at a strain of 3% to 6%.
[0012] Preferably, the sample is conditioned for 4 to 5 minutes, at a temperature of 100 to 110° C., at a frequency of 0.2 to 0.3 Hz, and at a strain of 4% to 5%.
[0013] Preferably, the frequency of the frequency scan is 0.1-20 Hz, the temperature is 80-130° C., and the strain is 2.8%-7%.
[0014] Preferably, the frequency of the frequency sweep is 0.1-20 Hz, the temperature is 90-120° C., and the strain is 3%-6%.
[0015] Preferably, the frequency of the frequency sweep is 0.1-20 Hz, the temperature is 100-110° C., and the strain is 4%-5%.
[0016] The present invention provides a method for testing the inherent molecular weight distribution type of natural rubber raw rubber, comprising the following steps: using a rotorless shear rheometer, subjecting the natural rubber raw rubber to sample adjustment and frequency scanning in sequence, and obtaining a series of scanning frequencies and loss moduli; using the scanning frequency as a logarithmic horizontal coordinate and the loss modulus as a logarithmic vertical coordinate, establishing a logarithmic relationship curve between the loss modulus and the scanning frequency; determining the inherent molecular weight distribution type of the natural rubber raw rubber through the relationship curve between the loss modulus and the scanning frequency: when the loss modulus increases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is bimodal; when the loss modulus decreases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is unimodal. The testing method of the present invention adopts a rheological method for testing, uses solid raw rubber as a sample, does not require liquid phase separation, and achieves the purpose of identifying the inherent molecular weight distribution type of natural rubber raw rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV in Example 1;
[0018] Figure 2 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV in Example 1;
[0019] Figure 3 is a logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV in Example 2;
[0020] Figure 4 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV in Example 2;
[0021] Figure 5 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV in Example 3;
[0022] Figure 6 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV in Example 3;
[0023] Figure 7 The chromatograms of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV in Comparative Example 1;
[0024] Figure 8 This is the chromatogram of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV in Comparative Example 1. DETAILED DESCRIPTION
[0025] The present invention provides a method for testing the inherent molecular weight distribution type of natural rubber raw rubber, comprising the following steps:
[0026] Using a rotorless shear rheometer, the natural rubber raw rubber was subjected to sample conditioning and frequency scanning in sequence to obtain a series of scanning frequencies and loss moduli;
[0027] With the scanning frequency as the logarithmic abscissa and the loss modulus as the logarithmic ordinate, a logarithmic relationship curve between the loss modulus and the scanning frequency is established;
[0028] The inherent molecular weight distribution type of the natural rubber raw rubber is determined by the relationship curve between the loss modulus and the scanning frequency: when the loss modulus increases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is bimodal; when the loss modulus decreases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is unimodal.
[0029] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0030] The present invention adopts a rotorless shear rheometer to sequentially perform sample adjustment and frequency scanning on natural rubber raw rubber to obtain a series of scanning frequencies and loss moduli.
[0031] In the present invention, the natural rubber raw rubber is preferably natural rubber raw rubber that has not been roller-molded.
[0032] In the present invention, the amount of the natural rubber raw rubber is preferably 4.0 to 5.0 g.
[0033] In the present invention, the sample adjustment time is preferably 2 to 8 minutes, more preferably 3 to 7 minutes, and most preferably 4 to 5 minutes; the temperature is preferably 80 to 130°C, more preferably 90 to 120°C, and most preferably 100 to 110°C; the frequency is preferably 0.1 to 0.5 Hz, more preferably 0.1 to 0.4 Hz, and most preferably 0.2 to 0.3 Hz; the strain is preferably 2.8% to 7%, more preferably 3% to 6%, and most preferably 4% to 5%.
[0034] In the present invention, the frequency of the frequency sweep is preferably 0.1-20 Hz; the temperature is preferably 80-130°C, more preferably 90-120°C, and most preferably 100-110°C; the strain is preferably 2.8%-7%, more preferably 3%-6%, and most preferably 4%-5%.
[0035] In the present invention, the logarithm in the logarithmic relationship curve between the loss modulus and the scanning frequency is preferably log10.
[0036] The test method for the inherent molecular weight distribution type of the natural rubber raw rubber provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0037] The test objects of Examples 1 to 3 and Comparative Example 1 were all IAN873 (IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV) of the "single-peak family" and Reyan73397 (Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV) of the "double-peak family";
[0038] Preparation of IAN873-RSS: take fresh latex of IAN873 → filter → take 45kg and pour into 100kg plug-in coagulation tank → add water to dilute (control the coagulation concentration to 15%) → add acid to coagulate (use 1.5% formic acid solution, the amount of acid is calculated according to neutralizing acid + 0.4% coagulation acid) → stir evenly, plug-in → mature for 5h → tablet → soak for 2h → dry the tablet and drip water for 2d → smoke dry (45℃×1d+60℃×3d);
[0039] Preparation of IAN873-RSSCV: take fresh latex of IAN873 → filter → take 45kg and pour into 100kg plug-in coagulation tank → add water to dilute (control the coagulation concentration to 15%) → add constant viscosity agent NHS (prepared into 5% aqueous solution) → add acid to coagulate (use 1.5% formic acid solution, the amount of acid is calculated according to neutralizing acid + 0.4% coagulation acid) → stir evenly, plug-in → mature for 5h → tablet → soak for 2h → dry the tablet and drip water for 2d → smoke dry (45℃×1d+60℃×3d);
[0040] Preparation of IAN873-TSR: Take fresh latex of Reyan73397 → filter → take 45kg and pour into a plastic basin of more than 80kg → dilute with water (control the coagulation concentration to 20%) → add acid to coagulate (use 3% formic acid solution, calculate the amount of acid according to neutralizing acid + 0.4% coagulation acid) → stir evenly → mature for 16h → press, crepe, tear into particles → dry in an oven at 83℃;
[0041] Preparation of IAN873-TSRCV: take fresh latex of IAN873 → filter → take 45kg and pour into a plastic basin with more than 80kg → dilute with water (control the coagulation concentration to 20%) → add constant viscosity agent NHS (configured into 5% aqueous solution) → add acid to coagulate (use 3% formic acid solution, the amount of acid is calculated according to neutralizing acid + 0.4% coagulation acid) → stir evenly → mature for 16h → press, crepe, tear into particles → dry in an oven at 83℃;
[0042] Preparation of Reyan73397-RSS: take fresh latex of Reyan73397 → filter → take 45kg and pour into 100kg plug-in coagulation tank → dilute with water (control the coagulation concentration at 15%) → add acid for coagulation (use 1.5% formic acid solution, calculate the amount of acid as neutralizing acid + 0.4% coagulation acid) → stir evenly, plug-in → mature for 5h → tablet → soak for 2h → dry the tablet and drip water for 2d → smoke dry (45℃×1d+60℃×3d);
[0043] Preparation of Reyan73397-RSSCV: take fresh latex of Reyan73397 → filter → take 45kg and pour into 100kg plug-in coagulation tank → dilute with water (control the coagulation concentration at 15%) → add acid for coagulation (use 1.5% formic acid solution, calculate the amount of acid as neutralizing acid + 0.4% coagulation acid) → stir evenly, plug-in → mature for 5h → tablet → soak for 2h → dry the tablet and drip water for 2d → smoke dry (45℃×1d+60℃×3d);
[0044] Preparation of Reyan73397-TSR: Take fresh latex of Reyan73397 → filter → take 45kg and pour into a plastic basin of more than 80kg → dilute with water (control the coagulation concentration to 20%) → add acid to coagulate (use 3% formic acid solution, calculate the amount of acid according to neutralizing acid + 0.4% coagulation acid) → stir evenly → mature for 16h → press, crepe, tear into particles → dry in an oven at 83℃;
[0045] Preparation of Reyan73397-TSRCV: take fresh latex of Reyan73397 → filter → take 45kg and pour into a plastic basin with more than 80kg → dilute with water (control the coagulation concentration at 20%) → add constant viscosity agent NHS (prepared into 5% aqueous solution) → add acid to coagulate (use 3% formic acid solution, and calculate the amount of acid based on neutralizing acid + 0.4% coagulating acid) → stir evenly → mature for 16h → press, crepe, tear into particles → dry in an oven at 83℃.
[0046] Example 1
[0047] 4.0g of IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV were weighed respectively and put into a rotorless shear rheometer for testing: the sample adjustment conditions were: frequency 0.5Hz, strain 2.8%, temperature 80℃, and time 8min; the frequency scanning conditions were: 0.1-20Hz, strain 7%, and temperature 80℃; the loss modulus G" (as shown in Table 1) under different frequency scans was recorded, and the scanning frequency was used as the logarithmic horizontal coordinate and the loss modulus G" was used as the logarithmic vertical coordinate to establish a logarithmic relationship curve between the scanning frequency and the loss modulus G" (as shown in Table 1). Figure 1 and Figure 2 As shown, Figure 1 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is shown in Figure 1. Figure 2 The logarithmic relationship curve (log10) between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV;
[0048] Table 1IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV
[0049] Loss modulus G" under different frequency sweeps
[0050]
[0051] Depend on Figures 1-2It can be seen that the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV decreases with increasing frequency, and the inherent molecular weight distribution type of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is unimodal, which is consistent with the actual situation; the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV increases with increasing frequency, and the inherent molecular weight distribution type of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV is bimodal, which is consistent with the actual situation.
[0052] Example 2
[0053] 4.0g of IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV were weighed respectively and put into a rotorless shear rheometer for testing: the sample adjustment conditions were: frequency of 0.5Hz, strain of 2.8%, temperature of 100℃, and time of 8min; the frequency scanning conditions were: 0.1-20Hz, strain of 7%, and temperature of 100℃; the loss modulus G" (as shown in Table 2) under different frequency scanning was recorded, and the scanning frequency was used as the logarithmic horizontal coordinate and the loss modulus G" was used as the logarithmic vertical coordinate to establish a logarithmic relationship curve between the scanning frequency and the loss modulus G" (as shown in Table 2). Figure 3 and Figure 4 As shown, Figure 3 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is shown in Figure 1. Figure 4 The logarithmic relationship curve (log10) between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV;
[0054] Table 2IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV
[0055] Loss modulus G" under different frequency sweeps
[0056]
[0057] Depend on Figures 3-4 It can be seen that the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV decreases with increasing frequency, and the inherent molecular weight distribution type of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is unimodal, which is consistent with the actual situation; the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV increases with increasing frequency, and the inherent molecular weight distribution type of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV is bimodal, which is consistent with the actual situation.
[0058] Example 3
[0059] 4.0g of IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV were weighed respectively and put into a rotorless shear rheometer for testing: the sample adjustment conditions were: frequency of 0.5Hz, strain of 2.8%, temperature of 130℃, and time of 8min; the frequency scanning conditions were: 0.1-20Hz, strain of 7%, and temperature of 130℃; the loss modulus G" (as shown in Table 3) under different frequency scanning was recorded, and the scanning frequency was used as the logarithmic horizontal coordinate and the loss modulus G" was used as the logarithmic vertical coordinate to establish a logarithmic relationship curve between the scanning frequency and the loss modulus G" (as shown in Table 3). Figure 5 and Figure 6 As shown, Figure 5 The logarithmic relationship curve between the scanning frequency and the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is shown in Figure 1. Figure 6 The logarithmic relationship curve (log10) between the scanning frequency and the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV;
[0060] Table 3IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV
[0061] Loss modulus G" under different frequency sweeps
[0062]
[0063] Depend on Figures 5-6 It can be seen that the loss modulus G" of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV decreases with increasing frequency, and the inherent molecular weight distribution type of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV is unimodal, which is consistent with the actual situation; the loss modulus G" of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV increases with increasing frequency, and the inherent molecular weight distribution type of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV is bimodal, which is consistent with the actual situation.
[0064] Comparative Example 1
[0065] Gel permeation chromatography (GPC) was used to characterize the molecular weight distribution of IAN873-RSS, IAN873-RSSCV, IAN873-TSR, IAN873-TSRCV, Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV. The test method was based on ISO16564-2004. The supernatant retained from the gel content test was filtered with a 1μm filter membrane and injected into a 2mL brown sample bottle. The molecular weight distribution was tested using a gel permeation chromatography. The test conditions were: THF was used as the eluent, the column oven temperature was 40°C, the injection volume was 100μL, and the flow rate was 1.0mL / min. The test results are as follows: Figures 7-8 As shown, Figure 7 The chromatograms of IAN873-RSS, IAN873-RSSCV, IAN873-TSR and IAN873-TSRCV are shown in Figure 1. Figure 8 is the chromatogram of Reyan73397-RSS, Reyan73397-RSSCV, Reyan73397-TSR and Reyan73397-TSRCV; Figures 7-8 It can be seen that the GPC test of the bimodal strain Reyan73397-RSS shows a unimodal distribution. Therefore, the present invention can trace the inherent molecular weight distribution of natural rubber, while the traditional method GPC test has errors.
[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for testing the inherent molecular weight distribution type of natural rubber raw rubber, characterized in that: The following steps are involved: Using a rotorless shear rheometer, the natural rubber raw rubber was subjected to sample conditioning and frequency scanning in sequence to obtain a series of scanning frequencies and loss moduli; With the scanning frequency as the logarithmic abscissa and the loss modulus as the logarithmic ordinate, a logarithmic relationship curve between the loss modulus and the scanning frequency is established; The inherent molecular weight distribution type of the natural rubber raw rubber is determined by the relationship curve between the loss modulus and the scanning frequency: when the loss modulus increases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is bimodal; when the loss modulus decreases with the increase of the scanning frequency, the inherent molecular weight distribution type of the natural rubber raw rubber is unimodal.
2. The testing method according to claim 1, characterized in that: The natural rubber raw rubber is natural rubber raw rubber that has not been roller-molded.
3. The testing method according to claim 1, characterized in that: The sample is conditioned for 2 to 8 minutes, at a temperature of 80 to 130° C., at a frequency of 0.1 to 0.5 Hz, and at a strain of 2.8% to 7%.
4. The testing method according to claim 3, characterized in that: The sample is conditioned for 3 to 7 minutes, at a temperature of 90 to 120° C., at a frequency of 0.1 to 0.4 Hz, and at a strain of 3% to 6%.
5. The testing method according to claim 4, characterized in that: The sample is conditioned for 4 to 5 minutes, at a temperature of 100 to 110° C., at a frequency of 0.2 to 0.3 Hz, and at a strain of 4% to 5%.
6. The testing method according to claim 1, characterized in that: The frequency of the frequency scanning is 0.1-20 Hz, the temperature is 80-130° C., and the strain is 2.8%-7%.
7. The testing method according to claim 6, characterized in that: The frequency of the frequency scanning is 0.1-20 Hz, the temperature is 90-120° C., and the strain is 3%-6%.
8. The testing method according to claim 7, characterized in that: The frequency of the frequency scanning is 0.1-20 Hz, the temperature is 100-110° C., and the strain is 4%-5%.
Citation Information
Patent Citations
Method for determining the molecular weight distribution in a polymer
CN101178348A
Method for detecting molecular weight of natural rubber
CN110501478A
Rheological method for comparing thermo-oxidative aging properties of raw natural rubber
CN116660507A
Pickering emulsion with stable WG-DNPs and application of Pickering emulsion in loading beta-carotene
CN117441876A