Hollow turbine blade precision casting simulation method based on ceramic core preheating deformation

By simulating the preheating deformation of ceramic core and mapping it into the solidification simulation of turbine blades, the problem of unconsidered impact of ceramic core preheating deformation on hollow turbine blade size in the prior art is solved, and a more accurate solidification simulation of turbine blades is achieved , improves dimensional accuracy.

CN119004884AActive Publication Date: 2024-11-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410986751.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-22
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing simulation technology fails to effectively consider the impact of ceramic core preheating deformation on the solidification size of hollow turbine blades, resulting in a large deviation from the actual measured data.

Method used

Simulation technology is used to simulate the thermal deformation of the ceramic core in a preheating environment, and its deformation state is mapped to the initial state of solidification simulation of the turbine blades. Numerical simulation is performed through the finite element analysis software ProCAST to generate the shell and creep deformation solution. , extract and map the creep results into the solidification simulation model, perform boundary conditions setting and material assignment, and perform blade solidification simulation.

Benefits of technology

It improves the accuracy of turbine blade solidification simulation, reduces the dimensional deviation caused by preheating deformation of ceramic core, provides more reliable dimensional research data, and improves the dimensional accuracy of the blade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119004884A_ABST
    Figure CN119004884A_ABST
Patent Text Reader

Abstract

The invention discloses a hollow turbine blade precision casting simulation method based on preheating deformation of a ceramic core, belongs to the field of investment casting processes, and aims to solve the problem that the simulation size of a hollow turbine blade is inaccurate due to the fact that creep deformation generated by preheating of the ceramic core is not considered in simulation. The method mainly comprises the following steps: (1) generating a corresponding shell model according to a CAD (Computer Aided Design) model of a blade ceramic core model; (2) numerical simulation of preheating of the ceramic core in the furnace according with actual production is realized; (3) extracting a displacement field of the ceramic core caused by preheating, mapping the displacement field to an initial state of the ceramic core in blade solidification simulation, and performing solidification simulation of the turbine blade on the basis; and (4) comparing the solidification simulation results of the turbine blade considering the preheating process of the ceramic core and not considering the preheating process with the size deviation of the design model. According to the method, the size change of the blade can be predicted more accurately, and more reliable data is provided for research on the size deformation of the hollow turbine blade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention relates to a hollow turbine blade investment casting process, which is a new numerical simulation method that uses simulation means to simulate the preheating creep deformation of the ceramic core leading to the change in the solidification size of the turbine blade. Technical Background

[0002] As an important part of aircraft engines, hollow turbine blades must work under high temperature and high pressure for a long time, so complex internal cooling structures are required to extend their service life. Ceramic cores are key components used to form complex cold zone channels during the investment casting process of hollow turbine blades.

[0003] During the investment casting process of turbine blades, the casting temperature of single crystal alloy is 1550℃. The ceramic core is fixed in the shell in advance. In order to avoid casting defects caused by the large temperature difference between the core shell and the molten metal when the molten metal is poured into the shell, the ceramic core and shell need to be preheated before pouring the molten metal. During the preheating process, the ceramic core will creep due to the high temperature environment and its own gravity, which will affect the size of the subsequent turbine blade after casting and solidification. The previous simulation technology did not consider the effect of the preheating deformation of the ceramic core on the final size of the turbine blade, resulting in a large deviation between the simulation results and the measured blade size data. Therefore, it is necessary to propose an investment casting solidification simulation that considers the preheating process of the ceramic core. Summary of the invention

[0004] In order to more accurately predict the deformation of hollow turbine blades in investment casting, the present invention proposes a numerical simulation method for investment casting of hollow turbine blades that takes into account the preheating deformation of the ceramic core. Certain simulation techniques are used to simulate the thermal deformation of the ceramic core in a preheating environment, and the deformation state of the ceramic core is mapped to the initial state of the turbine blade solidification simulation, so that the deformation results of the predicted turbine blades are more consistent with the actual investment casting working conditions, providing more reliable data for the size research of hollow turbine blades.

[0005] The technical solution of the present invention to achieve the above-mentioned purpose includes the following steps:

[0006] Step 1

[0007] The designed CAD model is divided into 7 parts, namely blades, ceramic core, feeding section, crystal selector, runner, condensation plate, and the furnace body also needs to generate a shell. The steps to generate the shell are as follows:

[0008] [1] Export the seven CAD models from the 3D modeling software (UG) into PRT format files.

[0009] [2] The model exported from ug is simultaneously imported into Hypermesh software to divide the surface mesh, and the surface mesh is exported in out format.

[0010] [3] The out format file is imported into the casting finite element software (ProCAST), and the Shelling command is used in the software to generate a shell for the casting model based on the surface mesh.

[0011] [4] Based on the surface mesh in [3], generate a tetrahedral mesh for the finite element model. At this time, there will be 8 volumes in the software: blade, ceramic core, feeding section, crystal selector, casting system, condensate plate, furnace body, and shell.

[0012] [5] Save the finite element model in [4] as two files in vdb format.

[0013] Step 2

[0014] To achieve numerical simulation of preheating of ceramic core in furnace in accordance with actual production, the specific steps are as follows:

[0015] [1] Open the first vdb file and use the Delete command to delete the blades, feeding section, crystal selector, gating system, and condensate tray from the eight volumes in ProCAST in step 1, leaving only the ceramic core, shell, and furnace body.

[0016] [2] Use the Add Materials command to set the ceramic core material to elasto-viscoplastic material properties (Elasto-ViscoPlastic).

[0017] [3] The temperature of the furnace body is set to change from room temperature to 1550°C within 1 hour according to the actual preheating temperature. The initial temperature of the shell and ceramic core is set to room temperature.

[0018] [4] The heating method of the furnace body for the mold shell and the ceramic core is set to radiation heating.

[0019] [5] Set the corresponding simulation parameters and perform finite element solution of heating creep deformation.

[0020] Step 3

[0021] Map the ceramic core preheating deformation to the solidification simulation and complete the blade solidification casting simulation:

[0022] [1] Open the second vdb file, use the Extract command to extract the creep simulation results of the ceramic core obtained in step 2, and use the Mapping command to map the extracted creep deformation results (displacement field) to the ceramic core of the simulation model and set it as the initial temperature condition of the ceramic core. Set the initial temperature conditions for other bodies.

[0023] [2] Assign a material to each body.

[0024] [3] Set boundary conditions.

[0025] [4] Set the simulation parameters and submit the blade solidification calculation.

[0026] Step 4

[0027] The outer contour dimensions of the corresponding cross-section are extracted, and the deviations of the solidification simulation results and the design model dimensions of the turbine blades with and without considering the preheating process of the ceramic core are compared.

[0028] The expected effect of the present invention is: according to actual production, the solidification simulation of turbine blades with preheating deformation of ceramic cores is used to more accurately predict the deformation of hollow turbine blades caused by preheating deformation of ceramic cores, which is more in line with the size distribution of blades in actual state, and has certain guiding significance for improving the dimensional accuracy of turbine blades.

[0029] The present invention is further described below with reference to the accompanying drawings and examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the flow chart of the patent of this invention.

[0031] Figure 2 It is the assembly relationship diagram of the feeding section, crystal selector, condensation plate, blades, runner, and ceramic core.

[0032] Figure 3 is the generated shell.

[0033] Figure 4 Assembly drawing of ceramic core and shell.

[0034] Figure 5 It is the displacement field map of the ceramic core.

[0035] Figure 6 It is the measurement section selection diagram.

[0036] Figure 7 It is a comparison chart of the deviation between the simulation size and the design model size in section 1 with and without considering the preheating process.

[0037] Figure 8 It is a comparison diagram of the deviation between the simulation size and the design model size in section 2 with and without considering the preheating process.

[0038] Fig. 9 It is a comparison diagram of the deviation between the simulation size and the design model size in section 3 with and without considering the preheating process. DETAILED DESCRIPTION

[0039] The following is a detailed description of the examples of the present invention in conjunction with the accompanying drawings: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given. However, the protection scope of the present invention is not limited to the following examples. Taking a hollow turbine blade as an example, the specific implementation process of the present invention is as follows: Figure 1 As shown:

[0040] Step 1

[0041] The designed CAD model is divided into 7 parts, namely blades, ceramic core, feeding section, crystal selector, runner, condensation plate, and furnace body. At this time, it is also necessary to generate a shell. The steps to generate a shell are as follows:

[0042] [1] Export the seven CAD models from the 3D modeling software (UG) into PRT format files.

[0043] Figure 2 This is the assembly relationship diagram of the shrink section, crystal selector, condensation plate, blades, runner, and ceramic core.

[0044] [2] The model exported from ug is simultaneously imported into Hypermesh software to divide the surface mesh, and the surface mesh is exported in out format.

[0045] [3] The out format file is imported into the casting finite element software (ProCAST), and the Shelling command is used in the software to generate a shell for the casting model based on the surface mesh.

[0046] Figure 3 is the generated shell.

[0047] [4] Based on the surface mesh in [3], generate a tetrahedral mesh for the finite element model. At this time, there will be 8 volumes in the software: blade, ceramic core, feeding section, crystal selector, casting system, condensate plate, furnace body, and shell.

[0048] [5] Save the finite element model in [4] as two files in vdb format.

[0049] Step 2

[0050] To achieve the numerical simulation of preheating the medium-sized shell with ceramic core in the furnace in accordance with actual production, the specific steps are as follows:

[0051] [1] Open the first vdb file and use the Delete command to delete the blades, feeding section, crystal selector, gating system, and condensate tray from the eight volumes in ProCAST in step 1, leaving only the ceramic core, shell, and furnace body.

[0052] Figure 4It is the assembly drawing of the ceramic core and shell.

[0053] [2] Use the Add Materials command to set the ceramic core material to Elasto-ViscoPlastic.

[0054] [3] The temperature of the furnace is set to rise from room temperature to 1550°C within 1 hour according to the actual preheating conditions, and the initial temperature of the shell and ceramic core is set to room temperature.

[0055] [4] The heating method of the furnace body for the mold shell and the ceramic core is set to thermal radiation heating.

[0056] [5] Set the corresponding simulation parameters to solve the heating creep deformation.

[0057] Step 3

[0058] The preheating deformation of the ceramic core is mapped to the solidification simulation to complete the blade solidification casting simulation.

[0059] [1] Open the second vdb file, use the extract command to extract the creep simulation results of the ceramic core obtained in step 2, and use the mapping command to map the extracted creep results to the ceramic core of the simulation model and set them as the initial temperature conditions of the ceramic core. Set the initial temperature conditions for other bodies.

[0060] Figure 5 The method is to map the displacement field of the ceramic core after preheating to the ceramic core in the solidification simulation.

[0061] [2] Assign a material to each body.

[0062] [3] Set boundary conditions.

[0063] [4] Set the simulation parameters and submit the calculation.

[0064] Step 4

[0065] The outer contour dimensions of the corresponding cross-section are extracted, and the deviations of the solidification simulation results of the turbine blade with and without considering the ceramic core preheating process are compared with the design model dimensions.

[0066] Figure 6 Select the plot for the measurement section.

[0067] Figure 7-9 So Figure 6 The selected section is taken as the object, and the solidification simulation size of the blade with and without considering the preheating process is calculated, and the difference between the design model size is compared. Figure 7-9It can be seen that the blade solidification numerical simulation method based on ceramic core preheating deformation is more in line with the actual working conditions because the influence of ceramic core preheating deformation on blade solidification deformation is taken into account, making the simulation results closer to the design model. The average deviation of section 1 is reduced by 0.073mm, and the maximum deviation is reduced by 0.441mm; the average deviation of section 2 is reduced by 0.005mm, and the maximum deviation is reduced by 0.165mm; the average deviation of section 3 is reduced by 0.009mm, and the maximum deviation is reduced by 0.133mm. Therefore, the accuracy of the simulation can be effectively improved by the blade solidification numerical simulation method based on ceramic core preheating deformation.

Claims

1. A hollow turbine blade precision casting simulation method based on ceramic core preheating deformation, characterized in that Follow these steps: Step 1 The designed CAD model is divided into 7 parts, namely blades, ceramic core, feeding section, crystal selector, runner, condensation plate, and the furnace body also needs to generate a shell. The steps to generate the shell are as follows: [1] Export the seven CAD models from the 3D modeling software (UG) into PRT format files. [2] The model exported from ug is simultaneously imported into Hypermesh software to divide the surface mesh, and the surface mesh is exported in out format. [3] The out format file is imported into the casting finite element software (ProCAST), and the Shelling command is used in the software to generate a shell for the casting model based on the surface mesh. [4] Based on the surface mesh in [3], generate a tetrahedral mesh for the finite element model. At this time, there will be 8 volumes in the software: blade, ceramic core, feeding section, crystal selector, casting system, condensate plate, furnace body, and shell. [5] Save the finite element model in [4] as two files in vdb format. Step 2 To achieve numerical simulation of preheating of ceramic core in furnace in accordance with actual production, the specific steps are as follows: [1] Open the first vdb file and use the Delete command to delete the blades, feeding section, crystal selector, gating system, and condensate tray from the eight volumes in ProCAST in step 1, leaving only the ceramic core, shell, and furnace body. [2] Use the Add Materials command to set the ceramic core material to elasto-viscoplastic material properties (Elasto-ViscoPlastic). [3] The temperature of the furnace body is set to change from room temperature to 1550°C within 1 hour according to the actual preheating temperature. The initial temperature of the shell and ceramic core is set to room temperature. [4] The heating method of the furnace body for the mold shell and the ceramic core is set to radiation heating. [5] Set the corresponding simulation parameters and perform finite element solution of heating creep deformation. Step 3 Map the ceramic core preheating deformation to the solidification simulation and complete the blade solidification casting simulation: [1] Open the second vdb file, use the Extract command to extract the creep simulation results of the ceramic core obtained in step 2, and use the Mapping command to map the extracted creep deformation results (displacement field) to the ceramic core of the simulation model and set it as the initial temperature condition of the ceramic core. Set the initial temperature conditions for other bodies. [2] Assign a material to each body. [3] Set boundary conditions. [4] Set the simulation parameters and submit the blade solidification calculation. Step 4 The outer contour dimensions of the corresponding cross-section are extracted, and the deviations of the solidification simulation results of the turbine blade with and without considering the preheating process of the ceramic core are compared with the dimensions of the design model.

Citation Information

Patent Citations

  • Finite element modeling method based on real material microstructure

    CN104063902A

  • Integrated casting design method for controlling miscellaneous crystals of single crystal blade edge plate

    CN110083927A

  • Modified edge extraction method for point cloud model of ceramic core of aerial blade

    CN110097588A

  • Method and apparatus for correcting printhead, printhead corrected by this apparatus, and printing apparatus using this printhead

    CN1134885A

  • Electric arc material increasing method of martensitic stainless steel impeller blade

    CN117324724A