Application of self-supporting liquid crystal in electrically regulated ion transmission

By regulating charge under acidic and alkaline conditions by two-dimensional oriented nanochannels of self-supporting liquid crystal materials, the problems of poor mechanical properties of nanochannels and difficulty in large-area preparation are solved, and efficient electrical regulation of ion transmission and mechanical performance improvement are achieved.

CN119008070AActive Publication Date: 2024-11-22TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310578754.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing materials have poor mechanical properties when building nanochannels, making it difficult to achieve large-area preparation and effective electrically regulated ion transmission.

Method used

Self-supported liquid crystal material is used to control its phase state to be smectic or nematic phase to form a two-dimensional directional nanochannel, and the charge of the nanochannel is regulated under acidic and alkaline conditions to achieve electrical regulation of ion transport.

Benefits of technology

It achieves good electrical regulation ion transmission effect and mechanical properties, is suitable for large-scale preparation, and is simple and cheap in preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008070A_ABST
    Figure CN119008070A_ABST
Patent Text Reader

Abstract

The invention discloses an application of a self-supporting liquid crystal in electrically regulated ion transmission. According to the self-supporting liquid crystal and the preparation method thereof, the liquid crystal with a specific structure is used for electrically regulating and controlling ion transmission, the size of the transmembrane current can be effectively regulated and controlled through the voltage applied to the liquid crystal, and the self-supporting liquid crystal is simple in preparation method, low in cost and suitable for large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of intelligent polymer material energy, and more specifically, to the application of self-supporting liquid crystal in electrically controlled ion transport. Background Art

[0002] Biological nanochannels can be opened or closed under environmental stimuli and play a key role in normal cells and biological processes. Biological nanochannels have three basic transport functions, namely ion selectivity, ion rectification and ion gating properties. For example, the OmpF pore protein in Gram-negative bacteria integrates the above three basic ion transport functions into one, enabling it to protect cells from damage caused by changes in the external acid-base environment. Nanochannels in organisms are mostly phospholipid molecular layers that are easily affected by the external environment and have poor stability. Therefore, scientists use functional materials to construct bionic artificial nanochannels. For example, a conical nanochannel is etched on a polyethylene terephthalate substrate, and a charged responsive functional molecule or block copolymer is modified on the surface of the nanochannel to achieve a nanochannel that responds to pH, light, temperature, etc. However, the mechanical properties of the above materials are poor and cannot be prepared on a large scale. Therefore, it is urgent and necessary to find new materials to construct nanochannels. Summary of the invention

[0003] Based on the above facts, the purpose of the present invention is to provide a self-supporting liquid crystal for use in electrically controlled ion transport.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] Application of a self-supporting liquid crystal in electrically controlled ion transport.

[0006] Furthermore, the phase state of the self-supporting liquid crystal is a smectic phase or a nematic phase, and each layer structure of the self-supporting liquid crystal contains a two-dimensional oriented nanochannel, and the two-dimensional oriented nanochannel is positively charged under acidic conditions and negatively charged under alkaline conditions.

[0007] In this technical solution, self-supporting liquid crystal is used for electrically regulated ion transport for the first time, achieving good electrically regulated ion transport effect. The phase state of the self-supporting liquid crystal also affects its application effect in electrically regulated ion transport. In this technical solution, it is found that when the phase state of the self-supporting liquid crystal is a smectic phase or a nematic phase, it has a good electrically regulated ion transport effect. When the phase state of the self-supporting liquid crystal is a smectic phase, the ion rectification effect is best. Preferably, the phase state of the self-supporting liquid crystal is a smectic phase.

[0008] In a preferred example, the two-dimensional oriented nanochannel of the self-supporting liquid crystal contains carboxyl groups connected by hydrogen bonds, which can ensure that the two-dimensional oriented nanochannel is positively charged under acidic conditions and negatively charged under alkaline conditions, giving the material a good ion rectification effect, etc.

[0009] Furthermore, the size of the two-dimensional oriented nanochannel is between 1-10 nm. If the size of the nanochannel is too large or too small, it is not only difficult to prepare, but also disadvantageous to ion transmission.

[0010] Preferably, the size of the two-dimensional oriented nanochannel is 1-3 nm. Exemplarily, the size of the two-dimensional oriented nanochannel includes but is not limited to 2-3 nm.

[0011] Furthermore, the thickness of the self-supporting liquid crystal is 5-50 μm. During the preparation process, the thickness of the self-supporting smectic liquid crystal material can be controlled by changing the thickness of the spacer of the liquid crystal box. Exemplarily, the thickness of the self-supporting liquid crystal is 10 μm.

[0012] Furthermore, the self-supporting liquid crystal is applied to electrically regulated ion transport in the form of a polymer film.

[0013] Furthermore, the material of the self-supporting liquid crystal is an aromatic liquid crystal compound and / or an aliphatic liquid crystal compound.

[0014] Furthermore, the preparation of the self-supporting liquid crystal comprises the following steps:

[0015] 1) Assembling a glass sheet with a polyvinyl alcohol alignment layer into a liquid crystal cell;

[0016] 2) pouring a mixed system of liquid crystal monomer, crosslinking agent and photoinitiator into a liquid crystal cell at 90-110° C., preferably 105° C., and then cooling the system;

[0017] 3) Photopolymerization;

[0018] 4) Heating the system to 130-150° C. and maintaining the temperature for 5-20 minutes to finally obtain the self-supporting liquid crystal.

[0019] It should be noted that the self-supporting liquid crystal in the present technical solution can obtain different phases, such as nematic phase, by changing the polymerization temperature. Further, when the temperature of the system after cooling in step 2) is 94-96°C, a smectic phase liquid crystal is obtained; when the temperature of the system after cooling in step 2) is 104-106°C, a nematic phase liquid crystal is obtained.

[0020] The self-supporting liquid crystal prepared by this method also has good mechanical properties.

[0021] Furthermore, the liquid crystal box substrate is selected from ordinary glass, quartz or silicon. Then, a polyvinyl alcohol alignment layer is coated on the substrate.

[0022] Furthermore, the conditions for the photopolymerization are: 1-5 mW / cm 2 Polymerize with 365 nm light for 5-20 minutes.

[0023] Furthermore, the photoinitiator is photoinitiator 184.

[0024] Furthermore, the liquid crystal monomer is

[0025] Furthermore, the cross-linking agent is

[0026] Furthermore, the application comprises the following steps:

[0027] placing at least a portion of the first surface of the self-supporting liquid crystal in an acidic electrolyte so that the corresponding nanochannel portion is positively charged;

[0028] The corresponding position of the second surface of the self-supporting liquid crystal relative to the first surface is placed in an alkaline electrolyte, so that the corresponding nanochannel part is negatively charged.

[0029] By this method, ion rectification is achieved.

[0030] It can be understood that the first surface and the second surface of the self-supporting liquid crystal are two opposite surfaces, and their directions are perpendicular to the layers of each layer structure in the self-supporting liquid crystal.

[0031] Furthermore, the pH of the acidic electrolyte is 2-6, preferably 2-3, and more preferably 2.

[0032] Furthermore, the pH of the alkaline electrolyte is 8-12, preferably 10-11, and more preferably 11.

[0033] Furthermore, the electrolyte in the acidic electrolyte and the alkaline electrolyte is KCl with a concentration of 10 -3 ~10 -4 M can give the smectic liquid crystal film a good ion rectification effect. More preferably, it is 10 -4 M, at this time the above effect is better.

[0034] Furthermore, the application comprises the following steps:

[0035] placing at least a portion of the first surface of the self-supporting liquid crystal in an acidic electrolyte so that the corresponding nanochannel portion is positively charged;

[0036] Placing a corresponding position of the second surface of the self-supporting liquid crystal relative to the first surface in an alkaline electrolyte so that the corresponding nanochannel portion is negatively charged;

[0037] Maintain a constant voltage across both sides of the electrolytic cell;

[0038] A voltage is applied to the self-supporting liquid crystal, and the magnitude of the transmembrane current is regulated by changing the magnitude of the voltage.

[0039] Through this method, a good electrically regulated ion transport effect was obtained, and a reversible change in the magnitude of the transmembrane current was achieved.

[0040] It can be understood that the first surface and the second surface of the self-supporting liquid crystal are two opposite surfaces, and their directions are perpendicular to the layers of each layer structure in the self-supporting liquid crystal.

[0041] It is also understandable that the above steps can be achieved by placing the self-supporting liquid crystal in an electrolytic cell while ensuring that at least a portion of the first surface of the self-supporting liquid crystal is located in an acidic electrolyte and a corresponding portion of the second surface is located in an alkaline electrolyte.

[0042] Furthermore, the pH of the acidic electrolyte is 2-6, preferably 2-3, and more preferably 2.

[0043] Furthermore, the pH of the alkaline electrolyte is 8-12, preferably 10-11, and more preferably 11.

[0044] Furthermore, the electrolyte in the acidic electrolyte and the alkaline electrolyte is KCl, and the concentration is preferably 10 -6 M.

[0045] Furthermore, the constant voltage is 1V.

[0046] Furthermore, the voltage applied to the self-supporting liquid crystal is in the range of 0 V to 0.5 V. At this time, reversible transformation of the transmembrane current can be achieved, for example, reversible transformation from 0 μA to 5.8 μA.

[0047] The beneficial effects of the present invention are as follows:

[0048] In the present invention, it is realized for the first time that liquid crystals with specific structures are used in electrically controlled ion transport, and the magnitude of transmembrane current can be effectively controlled by applying voltage thereto. In addition, the preparation method of the self-supporting liquid crystal is simple, low-cost, and suitable for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0050] Figure 1 The macroscopic image, scanning electron microscope image, atomic force microscope image, transmission electron microscope image and nanoindentation data of the self-supporting smectic liquid crystal material prepared in Example 1 are shown.

[0051] Figure 2 The differential scanning calorimetry data and X-ray diffraction data of the self-supporting smectic liquid crystal material prepared in Example 1 are shown.

[0052] Figure 3The Zeta potential data, current-voltage curve and rectification ratio at different concentrations of the self-supporting smectic liquid crystal material prepared in Example 1 are shown.

[0053] Figure 4 The self-supporting smectic liquid crystal material prepared in Example 1 shows the reversible change of the transmembrane current under voltage regulation. DETAILED DESCRIPTION

[0054] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0055] It should be noted that the liquid crystal monomer 6OBA in the following embodiments refers to:

[0056]

[0057] Liquid crystal crosslinker C6H refers to:

[0058]

[0059] Example 1

[0060] Preparation of self-supporting smectic liquid crystal materials:

[0061] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0062] 2) C6H / 6OBA (weight ratio 1:9, the structural formulas of the two are as follows Figure 1 A mixed system of 2 mol % photoinitiator 184 (shown in A) and 2 mol % photoinitiator 184 was poured into a liquid crystal cell at 105° C., and then the system was cooled to 95° C.;

[0063] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0064] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0065] Mechanical strength and morphology characterization results of self-supporting smectic liquid crystal materials

[0066] The obtained self-supporting smectic liquid crystal material was subjected to mechanical property characterization tests, such as Figure 1As shown in B and C, B1 is a smectic liquid crystal material that can withstand the weight of a 50g weight and has good flexibility, B2 is a macroscopic display of a large-area smectic liquid crystal material, and C is the modulus and hardness of liquid crystal materials in different phases (smectic phase, nematic phase, isotropic phase) obtained by nanoindentation experiments. A 5cm×5cm large-area self-supporting smectic liquid crystal polymer film can be prepared and can withstand the weight of a 50g weight hanging. The nanoindentation data show that the modulus of the self-supporting smectic liquid crystal material is 0.6GPa and the hardness is 0.08GPa. Scanning electron microscope image ( Figure 1 (D) shows that the prepared smectic liquid crystal film is dense and continuous, with no cracks in the top layer and cross section of the film and a thickness of about 10 μm. The atomic force image of the smectic liquid crystal film ( Figure 1 (E)) shows that the membrane surface is smooth with a roughness of about 6nm. Transmission electron microscopy image ( Figure 1 (F)) shows that the membrane is rich in ordered / oriented nanochannels with a pore size of about 3nm. X-ray diffraction also shows that the pore size of the nanochannels inside the membrane is 2.9nm, which is consistent with the results observed by transmission electron microscopy ( Figure 2 (B)). Differential scanning calorimetry ( Figure 2 (A)) shows that the glass transition temperature of the film is 72°C and the phase transition temperature is 178°C.

[0067] Example 2

[0068] Characterization of the rectification properties of self-supporting smectic liquid crystal materials

[0069] The rectification performance of the self-supporting smectic liquid crystal material prepared in Example 1 was studied.

[0070] The self-supporting smectic liquid crystal material is placed in different pH environments (such as pH between 3-11, such as pH 3, 4, 5, 6, 6.5, 8, 9, 10.5, etc.), and it can be seen that the nanochannels in the self-supporting smectic liquid crystal material can be positively or negatively charged under acidic or alkaline conditions. For example, when pH = 3, the Zeta potential in the nanochannel is 16mV. When pH = 10.5, the Zeta potential in the nanochannel is -58mV ( Figure 3 (A)).

[0071] Testing the ion rectification performance of the self-supporting smectic liquid crystal material comprises the following steps:

[0072] placing at least a portion of the first surface of the self-supporting liquid crystal in a 10 -4 M KCl electrolyte, so that the corresponding nanochannel part is positively charged;

[0073] The corresponding position of the second surface of the self-supporting liquid crystal relative to the first surface is placed in a 10 -4 MKCl electrolyte, making the corresponding nanochannel part negatively charged.

[0074] Measure the current-voltage curve ( Figure 3 (B), where the applied voltages are -2V to 2V, with an interval of 0.25V. In the negative voltage range, there is a significant transmembrane current. For example, the current is -123μA at -2V. In the positive voltage range, the transmembrane current is almost 0. For example, the current is 2.5μA at 2V. The rectification ratio of the liquid crystal material in this state is about 50 ( Figure 3 (D)).

[0075] We further studied the ion rectification performance of liquid crystal materials at different concentrations (the method is the same as above, except that the concentration of electrolyte KCl is adjusted to 10 -6 M, 10 -5 M, 10 -4 M, 10 -3 The rectifying effect of liquid crystal materials is unimodal with the concentration of solution ( Figure 3 (C)). As can be seen from the figure, the thickness of the double layer and the size of the nanochannel are more matched in the appropriate electrolyte concentration, resulting in a better rectification effect.

[0076] Example 3

[0077] Self-supporting smectic liquid crystal materials electrically control ion transport:

[0078] The electrically controlled ion transport performance of the self-supporting smectic liquid crystal material prepared in Example 1 was studied. The experimental apparatus is as follows: Figure 4 (A) is shown. The method specifically comprises the following steps:

[0079] placing at least a portion of the first surface of the smectic liquid crystal material in a 10 -6 M KCl electrolyte, so that the corresponding nanochannel part is positively charged;

[0080] The corresponding positions of the first surface and the second surface of the smectic phase liquid crystal material are placed in a 10 - 6 In the MKCl electrolyte, the corresponding nanochannel part is made negatively charged;

[0081] At the same time, maintaining a 1V voltage on both sides of the electrolytic cell, applying a voltage of 0 to 0.5V (0V, 0.1V, 0.2V, 0.3V, 0.4V, 0.5V) on the smectic liquid crystal material can achieve a reversible change in the transmembrane current from 0μA to 5.8μA ( Figure 4(B)). Furthermore, applying a sinusoidal voltage to the smectic liquid crystal material can achieve multiple reversible changes in the transmembrane current from 0 μA to 5.5 μA ( Figure 4 (C)).

[0082] Example 4

[0083] Preparation of self-supporting smectic liquid crystal materials:

[0084] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0085] 2) a mixed system of C6H / 6OBA (weight ratio 3:7) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0086] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0087] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0088] Example 5

[0089] Preparation of self-supporting smectic liquid crystal materials:

[0090] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0091] 2) A mixed system of C6H / 6OBA (weight ratio 5:5) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0092] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0093] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0094] Example 6

[0095] Preparation of self-supporting smectic liquid crystal materials

[0096] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 5 μm);

[0097] 2) a mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0098] 3) Use 5mW / cm 2Polymerization was performed by 365 nm light irradiation for 5 min;

[0099] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0100] Example 7

[0101] Preparation of self-supporting smectic liquid crystal materials

[0102] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 20 μm);

[0103] 2) a mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0104] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0105] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0106] Example 8

[0107] Preparation of self-supporting smectic liquid crystal materials

[0108] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 30 μm);

[0109] 2) a mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0110] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0111] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0112] Example 9

[0113] Preparation of self-supporting nematic liquid crystal materials

[0114] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0115] 2) A mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 105°C;

[0116] 3) Use 5mW / cm2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0117] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0118] Example 10

[0119] Preparation of self-supporting smectic liquid crystal materials

[0120] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0121] 2) a mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was cooled to 95°C;

[0122] 3) Use 1mW / cm 2 Polymerization was performed at 365 nm for 20 min;

[0123] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting smectic liquid crystal material.

[0124] The electrically regulated ion transport properties of the self-supporting smectic liquid crystal materials of Examples 4 to 10 were tested according to the method of Example 3, and the results also showed good electrically regulated ion transport properties.

[0125] Embodiment 11

[0126] Preparation of self-supporting nematic liquid crystal materials:

[0127] 1) Assemble glass sheets with polyvinyl alcohol alignment layers into a liquid crystal cell (spacing 10 μm);

[0128] 2) a mixed system of C6H / 6OBA (weight ratio 1:9) and 2 mol% of photoinitiator 184 was poured into a liquid crystal cell at 105°C, and then the system was kept at 105°C;

[0129] 3) Use 5mW / cm 2 Polymerization was performed by 365 nm light irradiation for 5 min;

[0130] 4) The system was heated to 135° C. and maintained for 5 minutes to finally obtain a self-supporting nematic liquid crystal material.

[0131] Compared with the smectic phase liquid crystal material prepared in Example 1, under the same experimental conditions, the rectification ratio of the nematic phase liquid crystal material is only 20 ( Figure 3 (D)).

[0132] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. Application of self-supporting liquid crystal in electrically controlled ion transport.

2. The use according to claim 1, It is characterized in that The phase state of the self-supporting liquid crystal is a smectic phase or a nematic phase, preferably a smectic phase; The self-supporting liquid crystal comprises two-dimensional directional nanochannels between each layer structure, and the two-dimensional directional nanochannels are positively charged under acidic conditions and negatively charged under alkaline conditions.

3. The use according to claim 2, It is characterized in that The two-dimensional oriented nanochannel contains carboxyl groups connected by hydrogen bonds; Preferably, the size of the two-dimensional oriented nanochannel is between 1-10 nm, more preferably 1-3 nm.

4. The use according to claim 2, It is characterized in that The material of the self-supporting liquid crystal is an aromatic liquid crystal compound and / or an aliphatic liquid crystal compound.

5. The use according to claim 1 or 2, It is characterized in that The preparation of the self-supporting liquid crystal comprises the following steps: 1) Assembling a glass sheet with a polyvinyl alcohol alignment layer into a liquid crystal cell; 2) pouring a mixed system of liquid crystal monomer, crosslinking agent and photoinitiator into a liquid crystal cell at 90-110° C., and then cooling the system; 3) Photopolymerization; 4) Heating the system to 130-150° C. and maintaining the temperature for 5-20 minutes to finally obtain the self-supporting liquid crystal.

6. The use according to claim 5, It is characterized in that The temperature after cooling is 94-96°C or 104-106°C; Preferably, the conditions for the photopolymerization are: 1-5 mW / cm 2 Polymerize with 365 nm light for 5-20 minutes.

7. The use according to any one of claims 1 to 3, It is characterized in that The steps include: placing at least a portion of the first surface of the self-supporting liquid crystal in an acidic electrolyte so that the corresponding nanochannel portion is positively charged; The corresponding position of the second surface of the self-supporting liquid crystal relative to the first surface is placed in an alkaline electrolyte, so that the corresponding nanochannel part is negatively charged.

8. The use according to claim 7, It is characterized in that The pH of the acidic electrolyte is 2-6, preferably 2; and / or The pH of the alkaline electrolyte is 8-12, preferably 11; and / or the electrolyte in the acidic electrolyte and the alkaline electrolyte is KCl with a concentration of 10 -3 ~10 -4 M, preferably 10 -4 M.

9. The use according to any one of claims 1 to 3, It is characterized in that The steps include: placing at least a portion of the first surface of the self-supporting liquid crystal in an acidic electrolyte so that the corresponding nanochannel portion is positively charged; Placing a corresponding position of the second surface of the self-supporting liquid crystal relative to the first surface in an alkaline electrolyte so that the corresponding nanochannel portion is negatively charged; Maintain a constant voltage across both sides of the electrolytic cell; A voltage is applied to the self-supporting liquid crystal, and the magnitude of the transmembrane current is regulated by changing the magnitude of the voltage.

10. The use according to claim 9, It is characterized in that The pH of the acidic electrolyte is 2-6, preferably 2; and / or The pH of the alkaline electrolyte is 8-12, preferably 11; and / or the electrolyte in the acidic electrolyte and the alkaline electrolyte is KCl with a concentration of 10 -6 M.

Citation Information

Patent Citations

  • Self-supporting blue-phase liquid crystal film and preparation method thereof

    CN111665653A

  • Preparation method of solid electrolyte film of anisotropic ion transmission channel

    CN114400372A

  • Liquid crystal electrolyte membrane, actuator, piezoelectric element, and stress sensor

    JP2022173845A

  • Liquid crystal-templated conducting organic polymers