Electrode paste and preparation method thereof
By using anode grooved powder and modified electrode paste, the problems of high ash content, high resistivity and low compressive strength of traditional electrode paste are solved, and electrode paste with low ash content, low resistivity and high mechanical strength are achieved, thereby improving the The stability and efficiency of the aluminum electrolysis process are achieved.
Patent Information
- Application Number
- CN202411117043.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional electrode pastes have problems such as high ash content, high resistivity and low compressive strength, which leads to unstable product quality and prone to soft or hard break accidents.
The anode grooved powder is used as the main component, and the physical structure of the electrode paste is optimized by filling the anode grooved powder with different particle sizes, combined with the modification treatment of tar, resin and adhesive, to improve the mechanical strength and electrical conductivity of the electrode paste.
The ash content and resistivity of the electrode paste are reduced, the mechanical strength and conductivity are improved, the soft or hard breaking phenomenon is reduced, and the durability and stability of the electrode are improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive materials, and in particular to an electrode paste and a preparation method thereof. Background Art
[0002] Electrode paste is a product of carbon products, also known as self-baking electrode. It is mainly used as conductive material in electric furnaces such as calcium carbide, ferroalloy, silicon-calcium alloy, and ferromanganese alloy. It is an important raw material in the electrolysis process of aluminum. In aluminum electrolytic cells, electrode paste is applied to carbon electrodes and serves as an important component of electrolyte.
[0003] The preparation of traditional electrode paste mainly uses anthracite, metallurgical coke, graphite powder, petroleum coke and asphalt coke as raw materials, and uses asphalt and coal tar as binders. It is usually a viscous black or brown substance. At present, the electrode paste products on the market generally have problems such as high ash content, high resistivity and low compressive strength, which leads to very unstable product quality and is prone to soft or hard breaks during use. Hard breaks are caused by insufficient strength of the electrode paste after sintering; soft breaks are caused by the electrode sintering speed being slower than the consumption speed, the electrode is lowered too quickly, and the electrode is not completely sintered and cannot withstand the stretching and lateral impact of the lower part of the electrode, resulting in breakage. Summary of the invention
[0004] In order to solve the above-mentioned problems, an electrode paste and a preparation method thereof are provided in an embodiment of the present application. The embodiment of the present application utilizes anode slotting powder as solid waste to prepare electrode paste, so that the prepared electrode paste has the advantages of low ash content, low resistivity and high mechanical strength.
[0005] To this end, the following technical solutions are adopted in the embodiments of the present application:
[0006] In a first aspect, an embodiment of the present application provides an electrode paste comprising the following components in parts by weight: 8-40 parts of anode slotting powder with a particle size below 0.075 mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1 mm, 20-35 parts of anode slotting powder with a particle size of 1-5 mm, 25-45 parts of aggregate, and 10-25 parts of asphalt; wherein the aggregate comprises anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 15-30:20-45:5-20:3-7:3-7.
[0007] In this embodiment, the anode slotting powder used is a carbonaceous powder produced by slotting the bottom of the anode carbon block before use in order to improve current efficiency, improve the stability of the electrolytic cell and reduce the cell voltage during the electrolytic aluminum production process. The fixed carbon content is between 90-98%, which is a high-value solid waste and can be used as a high-quality raw material for the production of high-quality electrode paste. Therefore, the electrode paste uses the above-mentioned anode slotting powder as the main component, which effectively reduces the ash content and helps to improve the purity and conductivity of the electrode paste.
[0008] In addition, anode slotting powders of different particle sizes can fill the gaps in the electrode paste, thereby optimizing the packing density of the electrode paste. Specifically, anode slotting powders with smaller particle sizes (below 0.075 mm): this part of the powder can fill the tiny gaps in the electrode paste, improve the density and uniformity of the electrode paste, and help improve the electrical conductivity and mechanical strength of the electrode paste; anode slotting powders with a particle size between 0.075-1 mm: these particles are relatively large and can fill larger gaps, increase the overall density of the electrode paste, and have a positive effect on the conductive properties of the electrolyte; anode slotting powders with a particle size between 1-5 mm: these larger particles are mainly used to increase the skeleton and mechanical strength of the electrode paste, effectively preventing soft or hard breakage of the electrode paste during use, and improving the durability and stability of the electrode.
[0009] Reasonable particle grading can effectively reduce the porosity of the electrode paste, thereby reducing resistivity and improving conductivity. Smaller particle size anode slotting powder fills tiny gaps, while larger particle size increases the overall mechanical strength. This combination enables the electrode paste to conduct current more stably and reliably during the electrolysis process. The advantage of using anode slotting powder of different particle sizes in the electrode paste is that it optimizes the physical structure of the electrode paste, improves its packing density and particle grading, thereby improving the electrolysis efficiency and the overall performance of the product.
[0010] Moreover, the main component of the aggregate used in the electrode paste is still the anode slotting powder. When preparing the aggregate, the anode slotting powder is modified with tar, resin and adhesive, which greatly enhances the mechanical strength of the prepared aggregate. The modified aggregate is added to the electrode paste to form the main skeleton of the electrode paste, thereby enhancing the mechanical strength of the electrode paste. At the same time, it is beneficial to improve the thermal shock resistance of the electrode paste product and reduce the linear expansion coefficient, thereby reducing quality accidents such as segregation, hard break or soft break during the use of the electrode paste.
[0011] As an achievable implementation method, the electrode paste includes the following components in parts by weight: 8-24 parts of anode slotting powder with a particle size of less than 0.075 mm, 20-24 parts of anode slotting powder with a particle size of 0.075-1 mm, 20-30 parts of anode slotting powder with a particle size of 1-5 mm, 38-45 parts of aggregate, and 10-18 parts of asphalt; wherein the aggregate includes anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 22-30:20-32:10-20:3-5:3-5.
[0012] As an achievable implementation method, the electrode paste includes the following components in parts by weight: 8 parts of anode slotting powder with a particle size of less than 0.075 mm, 20 parts of anode slotting powder with a particle size of 0.075-1 mm, 30 parts of anode slotting powder with a particle size of 1-5 mm, 38 parts of aggregate, and 10 parts of asphalt; wherein the aggregate includes anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 30:20:10:5:5.
[0013] In this embodiment, the applicant has optimized the selection and proportion of raw materials in the electrode paste after exploration, effectively reducing the ash content of the electrode paste, so that the resistivity of the electrode paste is effectively reduced, and at the same time, the mechanical strength of the electrode paste can be improved. The electrode paste with low resistivity can improve the conductivity of the electrolyte, which is conducive to improving production efficiency and reducing energy consumption. The electrode paste with high mechanical strength can reduce the quality accidents of soft or hard breaks.
[0014] As an achievable implementation, the resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1-5:2-7:3-8.
[0015] As an achievable implementation, the resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1-3:5-7:5-8.
[0016] As an achievable implementation, the resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1:5:8.
[0017] In this embodiment, the polyurethane resin generally has good adhesion and can effectively bond the anode slotting powder as a granular material. Moreover, the furan resin can provide good chemical stability in the aggregate, which contributes to the stability and corrosion resistance of the aggregate under different environmental conditions. At the same time, the phenolic resin generally has a higher hardness and excellent high temperature resistance, improves the structural stability of the aggregate, and facilitates the storage and transportation of the aggregate. The combined use of these resins can complement each other in the process of preparing the aggregate, thereby improving the overall performance of the electrode paste. The polyurethane resin provides adhesion and wear resistance, the furan resin enhances chemical stability and conductivity, and the phenolic resin enhances the hardness, temperature resistance and rigidity of the material. These advantages combined help to manufacture high-quality aggregates and ultimately improve the performance and life of the electrode paste. In this way, the reasonable changes in the components in the resin and the use of the above-mentioned ratio of resins are conducive to the production of high-quality aggregates, and then to the production of high-quality electrode paste.
[0018] As an achievable implementation, the adhesive includes at least one of anthracene oil and creosote oil.
[0019] In this embodiment, anthracene oil has excellent bonding properties and can effectively bond anode slotting powder and other components of different particle sizes together. This bonding property helps to improve the mechanical strength and stability of the electrode paste and reduce particle shedding or peeling during use.
[0020] As an achievable implementation method, the preparation method of the aggregate includes: taking 15-30 parts of anode slotting powder with a particle size of 0-1 mm, 20-45 parts of anode slotting powder with a particle size of 1-5 mm, 5-20 parts of tar, 3-7 parts of resin, and 3-7 parts of adhesive, stirring evenly and kneading, the kneading temperature is 150-250° C., and the kneading time is 1-3 hours; after the kneading is completed, pouring into a mold for pressing and molding, spray cooling and demolding; the demolded sample block is transported to a graphitization furnace and roasted at 2000-2200° C. for 15-20 hours, and taken out as the original aggregate block after cooling.
[0021] In this embodiment, by selecting anode slotting powder of different particle sizes, the particle gradation of the final aggregate can be regulated, thereby improving the mechanical strength of the aggregate, so that the aggregate as the skeleton of the electrode paste can improve the mechanical strength of the electrode paste. Tar is a brown oily product obtained by coal dry distillation. After dehydration, it is used for the preparation of aggregate. With resin and adhesive, it can well infiltrate and penetrate the surface and pores of anode slotting powder of various particle sizes, so that the particle components of various ingredients can be bonded to each other, so as to have good plasticity, facilitate mixing and compacting, and then improve the mechanical strength of the aggregate of the final fired product. The range of mixing temperature and time (150-250℃, 1-3 hours) can accurately control the curing process of the aggregate to ensure the molding quality and performance stability. The formed sample block is placed at a high temperature (2000-2200℃) for baking, which helps to improve the high temperature resistance and mechanical strength of the aggregate, making it suitable for use in high temperature environments. At the same time, the tar, resin and adhesive as additives are pyrolyzed and burned at high temperature, further reducing the ash content of the aggregate, so as to improve the conductivity and mechanical properties of the electrode paste made of the aggregate.
[0022] In some specific embodiments, the aggregate has a particle size of 5-13 mm.
[0023] In this embodiment, the larger aggregate particle size of 5-13 mm can constitute the skeleton of the electrode paste, which can provide good structural support and stability in the electrode paste and effectively increase the mechanical strength of the electrode paste.
[0024] In a second aspect, the present invention also provides a method for preparing an electrode paste, comprising the following steps:
[0025] Take 8-40 parts of anode slotting powder with a particle size of less than 0.075mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1mm, 20-35 parts of anode slotting powder with a particle size of 1-5mm, 25-45 parts of aggregate and 10-25 parts of asphalt, mix them evenly, then add them into a kneading pot for heating and kneading, the kneading temperature is 100-300℃, the kneading time is 1-3h, then pour the kneaded materials from the kneading pot, roll them in a mold, and obtain graphite conductive material product electrode paste after water cooling.
[0026] In some specific embodiments, the method for preparing the electrode paste comprises the following steps:
[0027] Step 1: Preparation of aggregate:
[0028] According to the required ratio of raw materials, take 15-30 parts of anode slotting powder with a particle size of 0-1mm, 20-45 parts of anode slotting powder with a particle size of 1-5mm, 5-20 parts of tar, 3-7 parts of resin, and 3-7 parts of adhesive, stir evenly and knead, the kneading temperature is 150-250℃, and the kneading time is 1-3h; after kneading, pour it into the mold for pressing and molding, spray cooling and demolding. The demolded sample block is transported to the graphitization furnace and roasted at 2000-2200℃ for 15-20h, and taken out as the original aggregate block after cooling;
[0029] Step 2: Preparation of raw materials:
[0030] Crushing the aggregate block obtained in step 1 into particles with a particle size of 5-13 mm as aggregate for later use;
[0031] Screening the anode slotting powder to screen out anode slotting powder granules with a particle size of 1-5 mm and anode slotting powder powder with a particle size of 0-1 mm, wherein a portion of the anode slotting powder with a particle size of 0-1 mm is ground into anode slotting powder with a particle size of less than 0.075 mm as fine powder for standby use;
[0032] Step 3: Prepare electrode paste:
[0033] 8-40 parts of anode slotting powder with a particle size of less than 0.075mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1mm, 20-35 parts of anode slotting powder with a particle size of 1-5mm, 25-45 parts of aggregate and 10-25 parts of asphalt are mixed evenly, then added into a kneading pot for heating and kneading, the kneading temperature is 100-300℃, the kneading time is 1-3h, and then the kneaded material is poured out of the kneading pot, roll-formed in a mold, and after water cooling, a graphite conductive material product electrode paste is obtained, which is stored in a finished product warehouse.
[0034] In this embodiment, the particle size distribution of aggregate and anode slotting powder can be accurately controlled by controlling the temperature and time during the kneading process, as well as the particle size control screening process, so as to optimize the conductive properties and rheological properties of the electrode paste; after the aggregate is subjected to high-temperature graphitization treatment, the stability and durability of the electrode paste in a high-temperature environment are improved, which is suitable for the needs of long-term high-temperature operation. The mechanical strength and corrosion resistance of the aggregate are enhanced by appropriate roasting temperature and time, so that the electrode paste can operate stably for a long time in a harsh environment. The stability of product quality and performance is guaranteed by optimizing the raw material ratio and preparation process. The preparation method of the present application uses anode slotting powder as solid waste as raw material, realizes the reuse of waste resources, conforms to the concept of sustainable development, and helps to save resources and reduce environmental pollution. At the same time, through precise raw material ratio and process control, a high-performance, high-temperature stable graphite conductive material product electrode paste preparation method is provided, which is suitable for applications requiring high conductivity and high temperature resistance.
[0035] In summary, the electrode paste and preparation method thereof provided in the embodiments of the present application have the advantages of reducing ash content, reducing resistivity, improving mechanical strength and comprehensive resource utilization, which are helpful to improve the quality stability problems existing in traditional electrode paste products and improve product performance. DETAILED DESCRIPTION
[0036] It is particularly noted that, unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The experimental reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the raw materials, instruments and equipment used in the following examples, etc., can all be purchased on the market or can be obtained by existing methods; the amounts of the experimental reagents used, unless otherwise specified, are the amounts of reagents used in conventional experimental operations; the experimental methods, unless otherwise specified, are all conventional methods.
[0037] Example 1
[0038] An electrode paste comprises the following components in parts by weight: 80 kg of anode slotting powder with a particle size of less than 0.075 mm, 200 kg of anode slotting powder with a particle size of 0.075-1 mm, 300 kg of anode slotting powder with a particle size of 1-5 mm, 380 kg of aggregate, and 100 kg of asphalt;
[0039] The aggregate comprises the following components in weight parts: 300 kg of anode slotting powder with a particle size of 0-1 mm, 200 kg of anode slotting powder with a particle size of 1-5 mm, 100 kg of tar, 50 kg of resin, and 50 kg of adhesive.
[0040] The anode slotting powder is a carbonaceous powder produced by slotting the bottom of the anode carbon block before use, and the fixed carbon content is between 90-98%. The resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1:5:8. The asphalt is a medium-grade viscosity asphalt between 60 and 300 Dow viscosity (that is, 0.06Pa·s to 0.3Pa·s), the softening point of the asphalt is 338-348k, and it is used after dehydration. The binder is anthracene oil. The particle size of the aggregate is 5-13mm.
[0041] It should be noted that particle size refers to the measurement of material size, usually expressed in mm, mesh, μm, etc. It can be determined by screening, that is, the particle size of the material is classified by sieve, and the material is also divided into aggregate and powder; the specification of the sieve is expressed by the aperture size, and the aperture size of a single sieve is consistent. An aperture size of 0.075mm is called a 0.075mm aperture sieve, and so on.
[0042] For example, a particle size of 0.075 mm or less refers to particles that can pass through a 0.075 mm sieve when sieving, and a particle size of 0.075-1 mm refers to particles that do not pass through a 0.075 mm sieve but pass through a 1 mm sieve when sieving.
[0043] For example, a particle size of 1-5 mm refers to particles that cannot pass through a sieve with a pore size of 1 mm but can pass through a sieve with a pore size of 5 mm when screening; a particle size of 5-13 mm refers to particles that cannot pass through a sieve with a pore size of 5 mm but can pass through a sieve with a pore size of 13 mm when screening.
[0044] According to the experimental research results, the main process of producing carbon conductive material from anode slot powder is determined as follows: prefabricated aggregate blocks of anode slot powder---roasting---crushing---mixing and molding---graphite conductive material products. Specifically, the above electrode paste is prepared by the following method:
[0045] Step 1: Preparation of aggregate:
[0046] Take 1000kg of anode slot powder from the bottom of the electrolytic cell of an aluminum plant in Northwest China, and after screening with a vibrating screen, get 550kg of 0-1mm anode slot powder and 450kg of 1-5mm anode slot powder. Weigh the powders separately: 300kg of 0-1mm anode slot powder, 200kg of 1-5mm anode slot powder, additives: 100kg of tar, 50kg of resin, 50kg of adhesive. Mix the above powders and additives in a stirrer and pour them into an electric heating kneading pot, set the kneading temperature to 150℃ and the kneading time to 1h. After kneading is completed, pour it into a mold and press it into a 100mm×600mm×900mm sample blank and spray cool it to demold it. After demolding, the sample is laid flat in a graphitization furnace and roasted at 2000℃ for 15h to obtain about 500kg of sintered aggregate blocks, and the additives are pyrolyzed and burned at high temperature.
[0047] Step 2: Preparation of raw materials:
[0048] The aggregate block obtained in step 1 is fed into a small jaw crusher and crushed into particles with a particle size of 5-13 mm as aggregate for standby use;
[0049] A drum screen device is used to screen the anode slotting powder, and anode slotting powder granules with a particle size of 1-5 mm and anode slotting powder powder with a particle size of 0-1 mm are screened out, wherein a portion of the 0-1 mm anode slotting powder powder is ground into anode slotting powder below 0.075 mm by a Raymond mill as fine powder for standby use, and at the same time, anode slotting powder powder with a particle size of 0.075-1 mm is screened out for standby use.
[0050] Step 3: Prepare electrode paste:
[0051] 80kg of anode slotting powder with a particle size of less than 0.075mm, 200kg of anode slotting powder with a particle size of 0.075-1mm, 300kg of anode slotting powder with a particle size of 1-5mm, 380kg of aggregate with a particle size of 5-13mm, and 100kg of asphalt are poured into a stirrer and stirred evenly, then added into a kneading pot and heated and kneaded at 200℃ for 2h. Then the kneaded materials are poured out of the kneading pot, rolled and formed in a mold, and pressed into 10mm×10mm×15mm. After water cooling, the graphite conductive material product electrode paste is obtained and stored in the finished product warehouse.
[0052] Example 2
[0053] Embodiment 2 also provides an electrode paste, which is different from Embodiment 1 in that the components constituting the electrode paste are different. Specifically, the electrode paste in Embodiment 2 includes the following components in parts by weight: 400 kg of anode slotting powder with a particle size of less than 0.075 mm, 350 kg of anode slotting powder with a particle size of 0.075-1 mm, 350 kg of anode slotting powder with a particle size of 1-5 mm, 450 kg of aggregate, and 250 kg of asphalt;
[0054] The aggregate comprises the following components in weight parts: 150 kg of anode slotting powder with a particle size of 0-1 mm, 450 kg of anode slotting powder with a particle size of 1-5 mm, 200 kg of tar, 70 kg of resin, and 70 kg of adhesive.
[0055] Example 3
[0056] Embodiment 3 also provides an electrode paste, which is different from Embodiment 1 in that the components constituting the electrode paste are different. Specifically, the electrode paste in Embodiment 3 includes the following components in weight parts: 240 kg of anode slotting powder with a particle size of less than 0.075 mm, 275 kg of anode slotting powder with a particle size of 0.075-1 mm, 275 kg of anode slotting powder with a particle size of 1-5 mm, 250 kg of aggregate, and 175 kg of asphalt;
[0057] The aggregate comprises the following components in weight parts: 225 kg of anode slotting powder with a particle size of 0-1 mm, 325 kg of anode slotting powder with a particle size of 1-5 mm, 50 kg of tar, 30 kg of resin, and 30 kg of adhesive.
[0058] Example 4
[0059] Example 4 also provides an electrode paste, which is different from Example 1 in that the resin used to prepare the aggregate is different. Specifically, the resin in Example 4 includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 3:2:5.
[0060] Example 5
[0061] Example 5 also provides an electrode paste, which is different from Example 1 in that the resin used to prepare the aggregate is different. Specifically, the resin in Example 5 includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 5:7:3.
[0062] Example 6
[0063] Example 6 also provides an electrode paste, which is different from Example 1 in that the resin used to prepare the aggregate is different. Specifically, the resin in Example 6 includes furan resin and phenolic resin in a weight ratio of 5:8.
[0064] Example 7
[0065] Example 7 also provides an electrode paste, which is different from Example 1 in that the resin used to prepare the aggregate is different. Specifically, the resin in Example 7 is phenolic resin.
[0066] Example 8
[0067] Example 8 also provides an electrode paste, which is different from Example 1 in that the resin used to prepare the aggregate is different. Specifically, the resin in Example 8 includes polyurethane resin, epoxy resin and phenolic resin in a weight ratio of 1:5:8.
[0068] Comparative Example 1
[0069] Comparative Example 1 also provides an electrode paste, which is different from Example 1 in that the components constituting the electrode paste are different. Specifically, the electrode paste in Comparative Example 1 includes the following components in parts by weight: 580 kg of anode slotting powder with a particle size of less than 0.075 mm, 380 kg of aggregate, and 100 kg of asphalt;
[0070] The aggregate comprises the following components in weight parts: 300 kg of anode slotting powder with a particle size of 0-1 mm, 200 kg of anode slotting powder with a particle size of 1-5 mm, 100 kg of tar, 50 kg of resin, and 50 kg of adhesive.
[0071] Comparative Example 2
[0072] Comparative Example 2 also provides an electrode paste, which is different from Example 1 in that the components constituting the electrode paste are different. Specifically, the electrode paste in Comparative Example 2 includes the following components in parts by weight: 580 kg of anode slotting powder with a particle size of 0.075-1 mm, 380 kg of aggregate, and 100 kg of asphalt;
[0073] The aggregate comprises the following components in weight parts: 300 kg of anode slotting powder with a particle size of 0-1 mm, 200 kg of anode slotting powder with a particle size of 1-5 mm, 100 kg of tar, 50 kg of resin, and 50 kg of adhesive.
[0074] Comparative Example 3
[0075] Comparative Example 3 also provides an electrode paste, which is different from Example 1 in that the components constituting the electrode paste are different. Specifically, the electrode paste in Comparative Example 3 includes the following components in parts by weight: 580 kg of anode slotting powder with a particle size of 1-5 mm, 380 kg of aggregate, and 100 kg of asphalt;
[0076] The aggregate comprises the following components in weight parts: 300 kg of anode slotting powder with a particle size of 0-1 mm, 200 kg of anode slotting powder with a particle size of 1-5 mm, 100 kg of tar, 50 kg of resin, and 50 kg of adhesive.
[0077] Comparative Example 4
[0078] Comparative Example 4 also provides an electrode paste, which is different from Example 1 in that the components for preparing the aggregate are different. Specifically, no resin is added during the preparation of the aggregate in Comparative Example 4.
[0079] Comparative Example 5
[0080] Comparative Example 5 also provides an electrode paste, which is different from Example 1 in that the components constituting the electrode paste are different. Specifically, the anode slotting powder in the electrode paste in Comparative Example 3 is completely replaced with calcined anthracite.
[0081] The electrode pastes obtained in the above examples and comparative examples were tested, and the testing method was based on the standard YB / T4448-2014. The physical and chemical indicators of the self-baking electrode paste for submerged arc furnace in YB / T4448-2014 are shown in Table 1:
[0082] Table 1 Physical and chemical indicators of self-baking electrode paste for submerged arc furnace in YB / T4448-2014
[0083]
[0084] Note: The elongation index is for reference only; recommended uses: Category 1 and 2 can be used for submerged arc furnaces with a power of ≥40MVA; Category 3 and 4 can be used for submerged arc furnaces with a power of 25-40MVA; Category 5 can be used for submerged arc furnaces of 25MVA and below.
[0085] The main technical indicators of 1-3 tests are shown in Table 2:
[0086] Table 2 Physical and chemical index test results of Examples 1-3
[0087]
[0088] As can be seen from Table 1 and Table 2, the ash content of the electrode paste obtained in Examples 1-8 is between 0.69-0.88%, the volatile matter is between 12.92-14.87%, the compressive strength is between 19.1-20.4 MPa, the resistivity is between 51-53 μΩ·m, and the volume density is between 1.45-1.49 g / cm 3 The elongation is between 10.3% and 13.6%. It meets the requirements of No. 1 electrode paste in the YB / T4448-2014 metallurgical industry standard, and some indicators are even better than the standard requirements.
[0089] It can be seen from Example 1 and Comparative Example 5 in combination with Table 2 that the electrode paste prepared by using anode slotting powder in the embodiments of the present application can significantly reduce the ash content of the electrode paste, thereby reducing the resistivity and improving the mechanical strength, compared with the calcined anthracite used in the traditional electrode paste.
[0090] It can be seen from Examples 1, 4-5 and Table 2 that although the aggregate is calcined at high temperature to remove all additives in the aggregate before preparing the electrode paste, the resin composition ratio of the aggregate prepared in the examples of the present application can still affect the compressive strength and elongation of the electrode paste. In addition, it can be seen from Examples 1, 6-8 and Comparative Example 4 and Table 2 that the lack of any component of the polyurethane resin, furan resin and phenolic resin in the constituent components of the resin (Examples 6-7) or any component is replaced by other resins (furan resin is replaced by epoxy resin in Example 8), or no resin is added to the aggregate (Comparative Example 4), will affect the compressive strength and elongation of the final finished electrode paste to a certain extent. This may be because the resin affects the performance of the aggregate during the high-temperature roasting process, so that after the aggregate is roasted at high temperature to form the original aggregate block, the physical and chemical indicators such as the ash content, volatile matter, bulk density, mechanical strength, and resistivity of the original aggregate block are optimized, and then the electrode paste is prepared using the aggregate after the roasting treatment, which can significantly improve the compressive strength of the electrode paste, reduce the ash content and make the volatile matter within a reasonable range. For example, through the reasonable change of the resin component, the friction between the materials can be overcome during the aggregate kneading and molding process, so that the material flow can be achieved and the particle size segregation can be reduced. The addition of resin is also conducive to the closer combination between the particles during the aggregate kneading and molding process, which is conducive to the improvement of the volume density of the green aggregate, the enhancement of the paste density, and the improvement of the compressive strength of the aggregate. At the same time, during the kneading process of the aggregate or powder paste and the aggregate, the kneading temperature or the aggregate temperature is increased to increase the temperature of the paste during the kneading process, and some gas is discharged, which is beneficial to reduce the amount of gas discharged during the solidification and baking of the green embryo, thereby improving the speed and quality of solidification, molding, and baking without generating cracks or bubbles, so that the volume density and compressive strength of the electrode paste are improved.
[0091] Through implementation 1-3 and comparative examples 1-3 and combined with Table 2, it can be seen that the compounding of continuous particle sizes used in the embodiments of the present application can significantly improve the compressive strength and volume density of the electrode paste compared to the anode slotting powder of a single particle size. This shows that the reasonable combination of anode slotting powders of different particle sizes can improve the volume density of the product, reduce the porosity, and increase the compressive strength, which conforms to the law of the most densely packed particles. Only adding anode slotting powder of a single particle size will reduce the volume density and compressive strength of the electrode paste. For example, in comparative example 1, which only adds anode slotting powder with a particle size of less than 0.075 mm, due to the fine particle size of the dust collecting powder, large specific surface area, and high adsorption capacity for asphalt, it will cause the porosity of the product to increase, thereby causing the volume density and compressive strength of the electrode paste to decrease.
[0092] Therefore, the embodiment of the present application proposes a method for preparing high-quality electrode paste using anode slot powder as raw material, which fully and reasonably utilizes the high fixed carbon content of anode slot powder and realizes the maximum resource utilization of solid waste. At the same time, the prepared electrode paste has low ash content, low resistivity, and high mechanical strength, which meets the increasingly high requirements of large-scale enclosed submerged arc furnaces for the quality of electrode paste. In addition, the selected raw materials are widely available, the preparation process is simple, the cost is low, and resource consumption is effectively reduced.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application. Those skilled in the art should understand that, although the present application is described in detail with reference to the aforementioned embodiments, the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions in the embodiments of the present application.
Claims
1. An electrode paste, characterized in that: It comprises the following components by weight: 8-40 parts of anode slotting powder with a particle size of less than 0.075mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1mm, 20-35 parts of anode slotting powder with a particle size of 1-5mm, 25-45 parts of aggregate, and 10-25 parts of asphalt; The aggregate comprises anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 15-30:20-45:5-20:3-7:3-7.
2. The electrode paste according to claim 1, characterized in that: It comprises the following components by weight: 8-24 parts of anode slotting powder with a particle size of less than 0.075mm, 20-24 parts of anode slotting powder with a particle size of 0.075-1mm, 20-30 parts of anode slotting powder with a particle size of 1-5mm, 38-45 parts of aggregate, and 10-18 parts of asphalt; The aggregate comprises anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 22-30:20-32:10-20:3-5:3-5.
3. The electrode paste according to claim 2, characterized in that: It comprises the following components by weight: 8 parts of anode slotting powder with a particle size of less than 0.075mm, 20 parts of anode slotting powder with a particle size of 0.075-1mm, 30 parts of anode slotting powder with a particle size of 1-5mm, 38 parts of aggregate, and 10 parts of asphalt; The aggregate comprises anode slotting powder with a particle size of 0-1 mm, anode slotting powder with a particle size of 1-5 mm, tar, resin and adhesive in a weight ratio of 30:20:10:5:
5.
4. The electrode paste according to any one of claims 1 to 3, characterized in that: The resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1-5:2-7:3-8.
5. The electrode paste according to claim 4, characterized in that: The resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1-3:5-7:5-8.
6. The electrode paste according to claim 5, characterized in that: The resin includes polyurethane resin, furan resin and phenolic resin in a weight ratio of 1:5:
8.
7. The electrode paste according to any one of claims 1 to 3, characterized in that: The adhesive includes at least one of anthracene oil and creosote oil.
8. The electrode paste according to claim 1, characterized in that: The particle size of the aggregate is 5-13 mm.
9. A method for preparing an electrode paste, characterized in that: The following steps are involved: Take 8-40 parts of anode slotting powder with a particle size of less than 0.075mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1mm, 20-35 parts of anode slotting powder with a particle size of 1-5mm, 25-45 parts of aggregate and 10-25 parts of asphalt, mix them evenly, then add them into a kneading pot for heating and kneading, the kneading temperature is 100-300℃, the kneading time is 1-3h, then pour the kneaded materials from the kneading pot, roll them in a mold, and obtain graphite conductive material product electrode paste after water cooling.
10. The method according to claim 9, characterized in that The following steps are also included: Step 1: Preparation of aggregate: According to the required ratio of raw materials, take 15-30 parts of anode slotting powder with a particle size of 0-1mm, 20-45 parts of anode slotting powder with a particle size of 1-5mm, 5-20 parts of tar, 3-7 parts of resin, and 3-7 parts of adhesive, stir evenly and knead, the kneading temperature is 150-250℃, and the kneading time is 1-3h; after kneading, pour it into the mold for pressing and molding, spray cooling and demolding. The demolded sample block is transported to the graphitization furnace and roasted at 2000-2200℃ for 15-20h, and taken out as the original aggregate block after cooling; Step 2: Preparation of raw materials: Crushing the aggregate block obtained in step 1 into particles with a particle size of 5-13 mm as aggregate for later use; Screening the anode slotting powder to screen out anode slotting powder granules with a particle size of 1-5 mm and anode slotting powder powder with a particle size of 0-1 mm, wherein a portion of the anode slotting powder with a particle size of 0-1 mm is ground into anode slotting powder with a particle size of less than 0.075 mm as fine powder for standby use; Step 3: Prepare electrode paste: Take 8-40 parts of anode slotting powder with a particle size of less than 0.075mm, 20-35 parts of anode slotting powder with a particle size of 0.075-1mm, 20-35 parts of anode slotting powder with a particle size of 1-5mm, 25-45 parts of aggregate and 10-25 parts of asphalt, mix them evenly, then add them into a kneading pot for heating and kneading, the kneading temperature is 100-300℃, the kneading time is 1-3h, then pour the kneaded materials from the kneading pot, roll them in a mold, and obtain graphite conductive material product electrode paste after water cooling.