IBC battery aluminum paste, IBC battery and preparation method of IBC battery
By using indium powder and lead/bismuth doped glass powder in IBC batteries, the aluminum paste is directly printed and sintered on the passivation layer, and the problem of battery open circuit voltage reduction caused by laser groove in the prior art is solved, and the battery is improved efficiency and open circuit voltage.
Patent Information
- Application Number
- CN202310573021.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-18
AI Technical Summary
The existing IBC batteries need to be laser grooved in the P+ area before printing into the positive gate line, resulting in the problem of lowering the open circuit voltage value of the battery cell.
Using an aluminum paste containing organic additives, boron powder, aluminum powder, indium powder and doped glass powder, the aluminum paste is directly printed on the passivation layer and carried out by adding indium powder and lead/bismuth doped glass powder to the aluminum paste. High-temperature sintering eliminates the laser groove step and improves the open circuit voltage and efficiency of the battery.
The damage to the passivation layer by laser groove is avoided, the open circuit voltage and contact probability of the battery is improved, and the side effects of aluminum are reduced. The silver aluminum corrosion pit formed is shallow and the composite is reduced, thereby improving the open circuit voltage and efficiency of the battery.
Smart Images

Figure CN119008075A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crystalline silicon solar cell manufacturing, and in particular to an IBC battery aluminum paste, an IBC battery and a preparation method thereof. Background Art
[0002] The interdigitated back contact (IBC) battery is a new type of battery in which the contact electrodes of the P / N junction, substrate and emitter region are made in an interdigitated shape on the back of the battery. Its core technology is to prepare high-quality p-regions and n-regions arranged in an interdigitated shape on the back of the battery.
[0003] At present, before printing the grid lines, P-type IBC batteries need to perform laser grooving on the P+ region to facilitate printing of aluminum paste to form positive electrode grid lines. However, laser grooving not only increases the production process, but also damages the passivation layer, resulting in a decrease in the open circuit voltage value of the battery. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an IBC battery aluminum paste, an IBC battery and a preparation method thereof, so as to solve the problem that before the existing IBC battery aluminum paste is printed into a positive electrode grid line, the P+ region needs to be laser grooved, resulting in a decrease in the open circuit voltage value of the battery cell.
[0005] In order to solve the above problems, the present invention is achieved through the following technical solutions:
[0006] The present invention proposes an IBC battery aluminum paste, wherein the components constituting the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth.
[0007] Furthermore, in the IBC battery aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.3-0.5%, 0.05-0.1%, 70-76%, 0.5-1%, 20.6-27.95% and 1.2-1.8%, respectively.
[0008] Furthermore, in the IBC battery aluminum paste, the doped glass powder is obtained by sintering and crushing 15 to 25 parts of Bi2O3, 6 to 8 parts of Al2O3, 10 to 25 parts of Pb2O5, 5 to 15 parts of ZnO, 10 to 15 parts of Sb2O5, 5 to 15 parts of V2O5, 12 to 20 parts of TiO2, and 12 to 20 parts of BaO, by mass.
[0009] Furthermore, in the IBC battery aluminum paste, the indium powder is micron-sized elemental indium.
[0010] Furthermore, in the IBC battery aluminum paste, the organic additive includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate mixture.
[0011] Furthermore, in the IBC battery aluminum paste, the organic binder includes a high molecular polymer resin and an organic solvent;
[0012] The mass fraction of the high molecular weight polymer in the organic binder is 9 to 14%;
[0013] The mass fraction of the organic solvent in the organic binder is 86-91%.
[0014] Furthermore, in the IBC battery aluminum paste, the high molecular polymer is ethyl cellulose-N20;
[0015] The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0016] Furthermore, in the IBC battery aluminum paste, the aluminum powder includes 85-90% by mass of micron spherical aluminum powder and 10-15% by mass of nano spherical aluminum powder.
[0017] The present invention also provides a method for preparing an IBC battery, which comprises:
[0018] After forming interdigitated n+ doped regions and p+ doped regions on the back of the silicon wafer, a passivation layer is formed on the surfaces of the n+ doped regions and the p+ doped regions;
[0019] Aluminum paste is printed on a first region of the passivation layer, and silver paste is printed on a second region of the passivation layer; a projection of the first region is within the range of the p+ doped region, and a projection of the second region is within the range of the n+ doped region; wherein the components constituting the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth;
[0020] The P-type silicon wafer with aluminum paste printed on the first area and silver paste printed on the second area is sintered at high temperature to produce an IBC battery.
[0021] The present invention also provides an IBC battery, wherein the IBC battery is prepared by the method as claimed in claim 9.
[0022] Compared with the prior art, the embodiments of the present invention have the following advantages:
[0023] In the embodiment of the present invention, the aluminum paste for IBC battery provided comprises organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth. By adding indium powder to the aluminum paste and using glass powder doped with lead and / or bismuth, indium and aluminum are both third main group elements and have similar chemical properties to aluminum, and indium, lead and bismuth have etching effects and high density. After forming a passivation layer on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then sintered at high temperature to contact with the p+ doped area and form a positive electrode grid line, eliminating the step of secondary laser grooving, avoiding damage to the passivation layer caused by the secondary laser grooving, and being able to increase the battery open circuit voltage; at the same time, during the sintering process The faster the aluminum drops to the silicon surface, the greater the chance of In-Si contact, reducing the contact resistance between the paste and the battery and maintaining a relatively high open circuit voltage. In addition, indium is used to replace part of the aluminum powder to reduce the aluminum content, which helps to reduce the side effects of Al, weakening the Al-Si reaction, forming shallower silver-aluminum corrosion pits and reducing recombination, thereby improving the battery's open circuit voltage and efficiency. This solves the problem that the existing IBC battery aluminum paste needs to be laser grooved in the P+ area before printing the positive grid line, resulting in a decrease in the open circuit voltage of the battery cell.
[0024] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a flow chart of a method for preparing IBC battery aluminum paste provided by an embodiment of the present invention;
[0026] Figure 2 It is a flow chart of the method for preparing an IBC battery provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] The applicant of the present invention has found that the main component of the metallization printing paste of the current P-type IBC is aluminum paste, which will cause great metal complexation to the battery cell itself, increase the series resistance of the battery cell, reduce the electrical performance of the battery cell itself, and lead to low opening voltage, large series resistance, and poor filling, which can easily affect the efficiency of the battery cell itself.
[0029] In order to solve the above problems, an embodiment of the present invention provides an IBC battery aluminum paste, wherein the components of the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth.
[0030] The IBC battery aluminum paste provided in the embodiment of the present invention is specifically an aluminum paste for forming a positive electrode grid line of a P-type IBC battery.
[0031] Among them, aluminum powder is the main component, and aluminum powder mainly replaces the P+ emitter of the battery, while indium has low resistance, good ductility, thermal conductivity, electrical conductivity and burn-through performance, and indium and aluminum are both third main group elements, and have similar chemical properties to aluminum. When the aluminum paste is printed on the passivation layer on the back of the silicon wafer, the silicon nitride film and silicon oxide film in the passivation layer can be burned through in sequence, and then contact with the p+ doped area to form a positive gate line, eliminating the step of secondary laser grooving and avoiding the damage of the passivation layer caused by the secondary laser grooving;
[0032] Among them, boron powder can diffuse into the silicon during high-temperature sintering for heavy doping, which is beneficial to improve the contact performance of the slurry and reduce the reaction contact surface between aluminum and silicon;
[0033] Among them, the doped glass powder is an inorganic adhesive, which will melt into liquid under high temperature conditions and condense when cooled to play a bonding role. The doped elements lead and bismuth have etching effects and high density. They can not only form a good aluminum-silicon alloy layer and P+ layer doping with silicon, but also penetrate into the aluminum grains to improve the material structure and increase the conductivity of the battery, thereby improving the efficiency of the battery. This solves the problem that the fine grid aluminum paste on the front of the existing N-type TOPCon battery is easily affected by the presence of aluminum elements and affects the battery efficiency; organic binders can ensure the overall bonding effect; and organic additives can reduce the overall viscosity of the silver paste.
[0034] Therefore, the aluminum paste provided in the embodiment of the present invention has better contact with the battery cell itself, and the series resistance is smaller than that of traditional aluminum paste. The recombination rate and degree of recombination will also be greatly improved, and the opening voltage of the battery can be increased by 5 millivolts, thereby solving the problem that the existing P-type IBC battery needs to perform laser grooving on the P+ area when printing the positive electrode grid line, resulting in a decrease in the open circuit voltage value of the battery cell.
[0035] Optionally, in one embodiment, in the aluminum paste, the mass percentage of organic additive is 0.3-0.5%; the mass percentage of boron powder is 0.05-0.1%; the mass percentage of aluminum powder is 70-76%; the mass percentage of indium powder is 0.5-1%; the mass percentage of organic binder is 20.6-27.95%; the mass percentage of doped glass powder is 1.2-1.8%. In the aluminum paste provided by the embodiment of the present invention, the aluminum content is relatively low. When forming aluminum silicon alloy, the proportion of aluminum in the aluminum silicon alloy is relatively small, so during the cooling process, no excess aluminum will diffuse into the PN junction area to form a metal composite area.
[0036] Optionally, in one embodiment, in the above-mentioned aluminum paste, the mass fractions of organic additives, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.35-0.45%, 0.06-0.08%, 72-75%, 0.6-0.8%, 23-26% and 1.35-1.45%, respectively.
[0037] For example, in the aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.3%, 0.1%, 70%, 0.5%, 27.95% and 1.15%, respectively.
[0038] For example, in the aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.5%, 0.05%, 76%, 1%, 21.25% and 1.2%, respectively.
[0039] For example, in the aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.5%, 0.1%, 76%, 1%, 20.6% and 1.8%, respectively.
[0040] For example, in the aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.4%, 0.06%, 72%, 0.5%, 25.54% and 1.5%, respectively.
[0041] For example, in the aluminum paste, the mass fractions of the organic additive, boron powder, aluminum powder, indium powder, organic binder and doped glass powder are 0.4%, 0.1%, 75%, 1%, 22% and 1.5%, respectively.
[0042] Optionally, in one embodiment, the indium powder is micron-grade elemental indium, specifically micron-grade elemental indium with a purity of 2 nines.
[0043] Optionally, in one embodiment, the boron powder includes micron-sized elemental boron. By adding the micron-sized elemental boron, the boron powder can quickly diffuse into the silicon for heavy doping during high-temperature sintering, which is beneficial to improving the contact performance of the slurry.
[0044] Optionally, in a specific embodiment, the boron powder is micron-grade boron powder with a purity of 3 9s.
[0045] Optionally, in another embodiment, the boron powder includes boron aluminum alloy. By adding the micron-sized boron aluminum alloy powder, the aluminum paste can quickly form a good alloy with silicon under a lower sintering temperature condition, thereby reducing the contact resistivity between the front aluminum fine grid and the battery.
[0046] Optionally, in one embodiment, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder, wherein there are gaps between the micron-sized aluminum powders, and the nano-sized spherical aluminum powder can just fill and penetrate into the gaps between the micron-sized aluminum powders.
[0047] Optionally, in a specific embodiment, the aluminum powder includes 85-90% by mass of micron-sized spherical aluminum powder and 10-15% by mass of nano-sized spherical aluminum powder.
[0048] Optionally, in a specific embodiment, the aluminum powder includes micron-sized spherical aluminum powder with a purity of 3 9s, a mass fraction of 85-95%, and a D50 of 5-6 μm, and nano-sized spherical aluminum powder with a purity of 3 9s, a mass fraction of 5-15%, and a D50 of 7-9 nm.
[0049] Optionally, in one embodiment, the organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, lauryl alcohol phosphate mixture, Digo 655, and BYKl09.
[0050] In the IBC battery aluminum paste provided in the embodiment of the present invention, the above-mentioned organic binder includes a polymer resin and an organic solvent; wherein the polymer resin is dissolved in the organic solvent, so that the organic solvent can be used as an organic binder, that is, the paste plays a role of bonding powder after drying.
[0051] Optionally, in one embodiment, the mass fraction of the high molecular weight polymer in the organic binder is 9 to 14%; the mass fraction of the organic solvent in the organic binder is 86 to 91%.
[0052] Optionally, in some embodiments, the mass fraction of the high molecular weight polymer in the organic binder is 10-12%; the mass fraction of the organic solvent in the organic binder is 88-90%.
[0053] Optionally, in one embodiment, the high molecular weight polymer is one or more of ethyl cellulose-N20, ethyl cellulose N-50, and ethyl cellulose-N100;
[0054] The organic solvent comprises at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0055] Optionally, in one embodiment, the glass powder is obtained by sintering and crushing 15-25 Bi2O3, 6-8 Al2O3, 10-25 Pb2O5, 5-15 ZnO, 10-15 Sb2O5, 5-15 V2O5, 12-20 TiO2, and 12-20 BaO, by weight, and the D50 of the glass powder is 1.2-1.8 μm. If the D50 is less than 1.2 μm, the glass activity is too large, and if the D50 is greater than 1.8 μm, the glass activity is too small. Optionally, the D50 of the glass powder is 1.5-1.8 μm.
[0056] Among them, Bi2O3 is the main network structure, ZnO can break the network structure and promote glass crystallization, Al2O3 can adjust the glass stability and increase the viscosity; Sb2O5 is used to clarify and uniform the glass liquid; Pb2O5 reacts with silicon nitride to produce lead, nitrogen and silicon dioxide, V2O5 and TiO2 can assist Pb2O5 and silicon nitride to react, and BaO is used for local crystallization.
[0057] The present invention also provides a method for preparing an IBC battery aluminum paste, wherein: Figure 1 As shown, it includes steps 101 to 102:
[0058] Step 101, mixing aluminum powder, boron powder, indium powder, an organic binder and doped glass powder to obtain a mixture; wherein the doping material of the doped glass powder is one or more of lead and bismuth;
[0059] Step 102: Grind the mixture, add an organic additive, and obtain IBC battery aluminum paste.
[0060] In the above step 101, 70-76% of aluminum powder, 0.05-0.1% of boron powder, 0.5-1% of indium powder, 20.6-27.95% of organic binder, and 1.2-1.8% of doped glass powder accounting for the total mass of the raw materials are weighed and mixed, and dispersed by a disperser to obtain the above mixture.
[0061] Optionally, in one embodiment, in the above step 101, the organic adhesive, nano-sized aluminum powder, boron powder and indium powder are first mixed and dispersed using a disperser, and then micron-sized aluminum powder and doped glass powder are added, dispersed again using a disperser, and then ground to obtain the above mixture.
[0062] In the above step 102, the above mixture is ground and then an organic additive accounting for 0.3-0.5% of the total mass of the raw materials is added. After high-speed dispersion, a positive electrode grid line that can contact the P+ area on the back of the IBC battery without laser grooving is obtained, thereby avoiding damage to the passivation layer caused by laser grooving.
[0063] In the embodiment of the present invention, by adding indium powder to aluminum paste and using glass powder doped with lead and / or bismuth, indium and aluminum are both third main group elements and have similar chemical properties to aluminum, and indium, lead and bismuth have etching effects and high density. After a passivation layer is formed on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then high-temperature sintering is performed to contact with the p+ doped area and form a positive grid line, eliminating the step of secondary laser grooving, avoiding damage to the passivation layer caused by the secondary laser grooving, and being able to improve the battery open circuit voltage; at the same time, during the sintering process, it drops to the silicon surface faster than aluminum, so that the In-Si contact probability is increased, the contact resistance between the slurry and the battery is reduced, and a higher open circuit voltage can be maintained; in addition, indium is used to replace part of the aluminum powder, the aluminum content is reduced, which is beneficial to reducing the side effects of Al, making the Al-Si reaction weaker, and the formed silver-aluminum corrosion pits are shallower and the composite is reduced, thereby improving the battery open circuit voltage and efficiency.
[0064] Optionally, in the preparation method provided in the embodiment of the present invention, the boron powder is micron-sized boron aluminum alloy and / or micron-sized elemental boron. Micron-sized boron aluminum alloy and micron-sized elemental boron have the characteristics of high tap density, low oxygen content and high activity. By adding the micron-sized boron aluminum alloy powder and / or micron-sized elemental boron, the aluminum paste can quickly form a good alloy with silicon under low sintering temperature conditions, thereby reducing the contact resistivity between the front aluminum fine grid and the battery.
[0065] Optionally, in the preparation method provided in an embodiment of the present invention, the organic additive includes two or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate.
[0066] Optionally, in the preparation method provided in the embodiment of the present invention, the silver powder includes 95-98% by mass of micron spherical silver powder and 2-5% by mass of nano spherical silver powder.
[0067] Optionally, in the preparation method provided in the embodiment of the present invention, the aluminum powder includes 85-95% by mass of micron spherical aluminum powder and 5-15% by mass of nano spherical aluminum powder.
[0068] Optionally, in the preparation method provided in an embodiment of the present invention, the doped glass powder is obtained by sintering and crushing 15 to 25 parts of Bi2O3, 6 to 8 parts of Al2O3, 10 to 25 parts of Pb2O5, 5 to 15 parts of ZnO, 10 to 15 parts of Sb2O5, 5 to 15 parts of V2O5, 12 to 20 parts of TiO2, and 12 to 20 parts of BaO, in parts by mass.
[0069] Optionally, in the preparation method provided in the embodiment of the present invention, the indium powder is micron-sized elemental indium.
[0070] Optionally, in the preparation method provided in an embodiment of the present invention, the organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate mixture.
[0071] Optionally, in the preparation method provided in the embodiment of the present invention, the organic binder comprises a high molecular polymer resin and an organic solvent;
[0072] The mass fraction of the high molecular weight polymer in the organic binder is 9 to 14%;
[0073] The mass fraction of the organic solvent in the organic binder is 86-91%.
[0074] Optionally, in the preparation method provided in the embodiment of the present invention, the high molecular polymer is ethyl cellulose-N20;
[0075] The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0076] Optionally, in the preparation method provided in the embodiment of the present invention, the aluminum powder includes 85-90% by mass of micron spherical aluminum powder and 10-15% by mass of nano spherical aluminum powder.
[0077] The present invention also provides a method for preparing an IBC battery, wherein: Figure 2 As shown, it includes steps 201 to 203:
[0078] Step 201, after forming interdigitated n+ doped regions and p+ doped regions on the back side of the silicon wafer, a passivation layer is formed on the surfaces of the n+ doped regions and the p+ doped regions;
[0079] Step 202, printing aluminum paste in the first area of the passivation layer, and printing silver paste in the second area of the passivation layer; the projection of the first area is within the range of the p+ doped area, and the projection of the second area is within the range of the n+ doped area; wherein the components constituting the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth;
[0080] Step 203: high-temperature sintering the P-type silicon wafer with aluminum paste printed on the first region and silver paste printed on the second region to obtain an IBC battery.
[0081] In the above step 201, the silicon wafer is firstly subjected to alkali texturing, and then an n+ doped region and a p+ doped region arranged in a finger-like manner are formed on the back of the silicon wafer, and then a silicon oxide layer or a silicon nitride layer is deposited to cover the entire back of the silicon wafer as the above passivation layer.
[0082] In the above step 202, the silicon wafer after forming the passivation layer is screen-printed to prepare the electrode grid lines. Specifically, the above aluminum paste is printed on the first area of the passivation layer on the back of the silicon wafer, and the projection of the first area is within the p+ doped area to form a positive grid line that is conductive with the p+ doped area; at the same time, it is also necessary to print silver paste on the second area of the back passivation layer, and the projection of the second area is within the n+ doped area to form a negative grid line spaced from the positive grid line, wherein the above silver paste can be a traditional silver paste.
[0083] In the above step 203, because indium powder is added to the aluminum paste and glass powder doped with lead and / or bismuth is used, indium and aluminum are both third main group elements and have similar chemical properties to aluminum, and indium, lead and bismuth have etching effects and high density. After the passivation layer is formed on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area and then sintered at high temperature, so that it can contact with the p+ doped area and form a positive grid line. There is no need for secondary laser grooving, which avoids damage to the passivation layer caused by the secondary laser grooving, and can improve the battery open circuit voltage; at the same time, during the sintering process, it drops to the silicon surface faster than aluminum, so that the In-Si contact probability is increased, the contact resistance between the slurry and the battery is reduced, and a higher open circuit voltage can be maintained; in addition, using indium to replace part of the aluminum powder reduces the aluminum content, which is beneficial to reducing the side effects of Al, weakening the Al-Si reaction, and forming a shallow silver-aluminum corrosion pit and reducing the composite, thereby improving the battery open circuit voltage and efficiency.
[0084] The silicon wafer may be an N-type silicon wafer or a P-type silicon wafer.
[0085] For example, when the silicon wafer is a P-type silicon wafer, step 101 specifically includes:
[0086] (1) Take a P-type original silicon wafer, and use low pressure chemical vapor deposition (LPCVD) to form an ultra-thin silicon oxide layer on the back of the P-type silicon wafer as an ultra-thin tunneling oxide layer, and then prepare a polysilicon layer with a thickness that can meet the passivation effect on both sides; because the double-sided preparation of the polysilicon layer is conducive to the subsequent removal of the front polysilicon layer, it is not easy to have the two extreme situations of excessive removal or insufficient removal, and the yield is better controlled;
[0087] (2) After the polysilicon layer is prepared, the silicon wafer is fed into a furnace tube to dope the polysilicon layer with phosphorus to form an n+ doped region;
[0088] (3) laser grooving the back of the silicon wafer to expose the p+ doped region, forming n+ doped regions and p+ doped regions arranged in an interdigitated manner, and then removing the front polysilicon layer by a wet method;
[0089] (4) Atomic layer deposition (ALD) is used to plate a passivation layer on the entire front and back of the product to form field passivation; after the aluminum oxide film is formed, an anti-reflection film is first plated on the front of the battery, and then on the back to further enhance the passivation effect of the battery cell.
[0090] The present invention is described in detail below by way of examples.
[0091] Example 1
[0092] (1) Providing aluminum paste a1: In parts by mass, the IBC battery aluminum paste a1 is composed of 0.4 parts of an organic additive, 72 parts of aluminum powder, 0.5 parts of elemental indium, 0.06 parts of boron powder, 25.54 parts of an organic binder and 1.5 parts of doped glass powder;
[0093] The organic additives include lauryl phosphate and a mixture of lauryl alcohol phosphate; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 9s and a mass fraction of 92%, and nano-spherical aluminum powder with a purity of 3 9s and a mass fraction of 8%; the organic binder includes 10% ethyl cellulose-N100 and 90% organic solvents, and the organic solvents include butyl carbitol, butyl carbitol acetate, Span 85 and alcohol ester twelve;
[0094] The doped glass powder is obtained by sintering and crushing 20 Bi2O3, 6 parts Al2O3, 12 parts Pb2O5, 10 parts ZnO, 12 parts Sb2O5, 10 parts V2O5, 15 parts TiO2 and 15 parts BaO.
[0095] (2) After forming a silicon oxide layer and a polysilicon layer in sequence on the back side of a P-type silicon wafer with a size of 182 mm×182 mm, phosphorus is doped into the back side polysilicon layer;
[0096] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0097] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a1 is printed on the back silicon nitride layer opposite to the p+ doped region by a 360-mesh screen, and a silver paste is printed on the back silicon nitride layer opposite to the n+ doped region;
[0098] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772°C, to produce a P-type IBC battery.
[0099] After sintering, the electrical properties tested were: open circuit voltage 0.7185V, short circuit current 13.825A, filling 83.5%, and photoelectric conversion efficiency 25.122%.
[0100] Example 2
[0101] (1) Providing aluminum paste a2: In parts by mass, the IBC battery aluminum paste a1 is composed of 0.4 parts of an organic additive, 75 parts of aluminum powder, 1 part of elemental indium, 0.1 parts of boron powder, 22 parts of an organic binder and 1.5 parts of doped glass powder;
[0102] The organic additives include lauryl phosphate and a mixture of lauryl alcohol phosphate; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 9s and a mass fraction of 90%, and nano-spherical aluminum powder with a purity of 3 9s and a mass fraction of 10%; the organic binder includes 10% ethyl cellulose-N100 and 90% organic solvent, and the organic solvent includes butyl carbitol, butyl carbitol acetate, Span 85 and alcohol ester twelve;
[0103] The doped glass powder is obtained by sintering and crushing 20 Bi2O3, 6 parts Al2O3, 12 parts Pb2O5, 10 parts ZnO, 12 parts Sb2O5, 10 parts V2O5, 15 parts TiO2 and 15 parts BaO.
[0104] (2) After forming a silicon oxide layer and a polysilicon layer in sequence on the back side of a P-type silicon wafer with a size of 182 mm×182 mm, phosphorus is doped into the back side polysilicon layer;
[0105] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0106] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a2 is printed on the back silicon nitride layer opposite to the p+ doped region by a 360-mesh screen, and a silver paste is printed on the back silicon nitride layer opposite to the n+ doped region;
[0107] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772°C, to produce a P-type IBC battery.
[0108] After sintering, the electrical properties tested were: open circuit voltage 0.719V, short circuit current 13.865A, filling 83.2%, and photoelectric conversion efficiency 25.12%.
[0109] Example 3
[0110] (1) providing aluminum paste a3: in parts by mass, the IBC battery aluminum paste a3 is composed of 0.4 parts of an organic additive, 72 parts of aluminum powder, 0.6 parts of elemental indium, 0.06 parts of boron powder, 25.54 parts of an organic binder and 1.4 parts of doped glass powder;
[0111] The organic additives include lauryl phosphate and lauryl alcohol phosphate; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 9s and a mass fraction of 92%, and nano-spherical aluminum powder with a purity of 3 9s and a mass fraction of 8%; the organic binder includes 10% ethyl cellulose-N100 and 90% organic solvent, and the organic solvent includes butyl carbitol, butyl carbitol acetate, Span 85 and alcohol ester twelve;
[0112] The doped glass powder is obtained by sintering and crushing 20 Bi2O3, 6 parts Al2O3, 12 parts Pb2O5, 10 parts ZnO, 12 parts Sb2O5, 10 parts V2O5, 15 parts TiO2 and 15 parts BaO.
[0113] (2) After forming a silicon oxide layer and a polysilicon layer on the back side of an N-type silicon wafer with a size of 182 mm×182 mm, the back side polysilicon layer is doped with boron;
[0114] (3) laser grooving the back side of the boron-doped N-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0115] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a3 is printed on the back silicon nitride layer opposite to the p+ doped region by a 360-mesh screen, and a silver paste is printed on the back silicon nitride layer opposite to the n+ doped region;
[0116] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772° C., to produce an N-type IBC battery.
[0117] After sintering, the electrical properties tested were: open circuit voltage 0.720V, short circuit current 13.855A, filling 83.15%, and photoelectric conversion efficiency 25.121%.
[0118] Comparative Example 1
[0119] (1) Providing aluminum paste b1: In parts by mass, the IBC battery aluminum paste b1 is composed of 0.4 parts of organic additive, 76 parts of aluminum powder, 0.1 parts of boron powder, 22 parts of organic binder and 1.5 parts of doped glass powder;
[0120] The organic additives include lauryl phosphate and lauryl alcohol phosphate; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 9s and a mass fraction of 90%, and nano-spherical aluminum powder with a purity of 3 9s and a mass fraction of 10%; the organic binder includes 10% ethyl cellulose-N100 and 90% organic solvent, and the organic solvent includes butyl carbitol, butyl carbitol acetate, Span 85 and alcohol ester twelve;
[0121] The doped glass powder is obtained by sintering and crushing 20 Bi2O3, 6 parts Al2O3, 12 parts MgO, 10 parts ZnO, 12 parts Sb2O5, 10 parts V2O5, 15 parts TiO2 and 15 parts BaO.
[0122] (2) After forming a silicon oxide layer and a polysilicon layer in sequence on the back side of a P-type silicon wafer with a size of 182 mm×182 mm, phosphorus is doped into the back side polysilicon layer;
[0123] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0124] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste b1 is printed on the back silicon nitride layer opposite to the p+ doped region by a 360-mesh screen, and a silver paste is printed on the back silicon nitride layer opposite to the n+ doped region;
[0125] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with the peak sintering temperature being 772° C., to produce an IBC battery.
[0126] After sintering, the electrical properties tested were: open circuit voltage of 0.7155V, short circuit current of 13.845A, filling of 83.32%, and photoelectric conversion efficiency of 25.000%.
[0127] Comparative Example 2
[0128] (1) Providing aluminum paste b2: In parts by mass, the IBC battery aluminum paste b2 is composed of 0.4 parts of an organic additive, 72.6 parts of elemental indium, 0.06 parts of boron powder, 25.54 parts of an organic binder and 1.4 parts of doped glass powder;
[0129] The organic additives include lauryl phosphate and lauryl alcohol phosphate; the aluminum powder includes micron-grade spherical aluminum powder with a purity of 3 9s and a mass fraction of 90%, and nano-spherical aluminum powder with a purity of 3 9s and a mass fraction of 10%; the organic binder includes 10% ethyl cellulose-N100 and 90% organic solvent, and the organic solvent includes butyl carbitol, butyl carbitol acetate, Span 85 and alcohol ester twelve;
[0130] The doped glass powder is obtained by sintering and crushing 20 Bi2O3, 6 parts Al2O3, 12 parts MgO, 10 parts ZnO, 12 parts Sb2O5, 10 parts V2O5, 15 parts TiO2 and 15 parts BaO.
[0131] (2) After forming a silicon oxide layer and a polysilicon layer on the back side of an N-type silicon wafer with a size of 182 mm×182 mm, the back side polysilicon layer is doped with boron;
[0132] (3) laser grooving the back side of the boron-doped N-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0133] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste b1 is printed on the back silicon nitride layer opposite to the p+ doped region by a 360-mesh screen, and a silver paste is printed on the back silicon nitride layer opposite to the n+ doped region;
[0134] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 772°C, to produce a P-type IBC battery.
[0135] After sintering, the electrical properties tested were: open circuit voltage of 0.7158V, short circuit current of 13.825A, filling of 83.45%, and photoelectric conversion efficiency of 25.013%.
[0136] By comparing Examples 1 to 2 with Comparative Example 1, and Example 3 with Comparative Example 2, it can be seen that by forming a P+ emitter using aluminum paste doped with indium, lead, and bismuth, a back pole grid line can be formed without laser grooving, and the recombination rate and degree of the battery will also be greatly improved, with the efficiency of the battery increased by 0.1% and the start-up voltage increased by 3mv.
[0137] In summary, in the present embodiment, by adding indium powder to the aluminum paste and using lead and / or bismuth doped glass powder, indium and aluminum are both third main group elements, have similar chemical properties to aluminum, and indium, lead and bismuth have etching effects and high density. After forming a passivation layer on the back of the battery silicon wafer, it is directly printed on the passivation layer area above the p+ doped area, and then sintered at a high temperature, it can contact with the p+ doped area and form a positive electrode grid line, eliminating the step of secondary laser grooving, avoiding the damage of the passivation layer caused by the secondary laser grooving, and can improve the battery open circuit voltage; at the same time, During the sintering process, aluminum drops to the silicon surface faster than indium, which increases the probability of In-Si contact, reduces the contact resistance between the slurry and the battery, and maintains a relatively high open circuit voltage. In addition, indium is used to replace part of the aluminum powder to reduce the aluminum content, which helps to reduce the side effects of Al, weaken the Al-Si reaction, and form shallower silver-aluminum corrosion pits and reduce recombination, thereby improving the open circuit voltage and efficiency of the battery. This solves the problem that the existing IBC battery aluminum paste needs to be laser grooved in the P+ area before printing the positive grid line, which leads to a decrease in the open circuit voltage of the battery cell.
[0138] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0139] The above is a detailed introduction to an IBC battery aluminum paste, an IBC battery and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. An IBC battery aluminum paste, characterized in that: The components constituting the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth.
2. The IBC battery aluminum paste according to claim 1, characterized in that: The mass fractions of the organic auxiliary agent, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder are 0.3-0.5%, 0.05-0.1%, 70-76%, 0.5-1%, 20.6-27.95% and 1.2-1.8% respectively.
3. The IBC battery aluminum paste according to claim 1, characterized in that: In parts by mass, the doped glass powder is obtained by sintering and crushing 15-25 parts of Bi2O3, 6-8 parts of Al2O3, 10-25 parts of Pb2O5, 5-15 parts of ZnO, 10-15 parts of Sb2O5, 5-15 parts of V2O5, 12-20 parts of TiO2, and 12-20 parts of BaO.
4. The IBC battery aluminum paste according to claim 1, characterized in that: The indium powder is micron-sized single substance indium.
5. The IBC battery aluminum paste according to claim 1, characterized in that: The organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, dibasic acid ester, and lauryl alcohol phosphate mixture.
6. The IBC battery aluminum paste according to claim 5, characterized in that: The organic binder includes a high molecular polymer resin and an organic solvent; The mass fraction of the high molecular weight polymer in the organic binder is 9 to 14%; The mass fraction of the organic solvent in the organic binder is 86-91%.
7. The IBC battery aluminum paste according to claim 6, characterized in that: The high molecular polymer is ethyl cellulose-N20; The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
8. The IBC battery aluminum paste according to claim 1, characterized in that: The aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder.
9. A method for preparing an IBC battery, characterized in that: include: After forming interdigitated n+ doped regions and p+ doped regions on the back of the silicon wafer, a passivation layer is formed on the surfaces of the n+ doped regions and the p+ doped regions; Printing aluminum paste on a first region of the passivation layer, and printing silver paste on a second region of the passivation layer; The projection of the first region is within the range of the p+ doped region, and the projection of the second region is within the range of the n+ doped region; wherein the components constituting the aluminum paste include organic additives, boron powder, aluminum powder, indium powder, organic adhesive and doped glass powder, and the doping material of the doped glass powder is one or more of lead and bismuth; The P-type silicon wafer with aluminum paste printed on the first area and silver paste printed on the second area is sintered at high temperature to produce an IBC battery.
10. An IBC battery, characterized in that: The method according to claim 9 is used to prepare the product.
Citation Information
Patent Citations
Conductive paste for solar cell and preparation method of conductive paste
CN105679400A
High-performance solar front conductive silver paste and preparation method thereof
CN112825276A
Front aluminum paste suitable for N-type TOPCon battery and preparation method of front aluminum paste
CN114203335A
Type of front finger paste for n-type solar cells as well as its preparation methods
US20220238249A1