High-orientation-degree sintered neodymium-iron-boron rare earth permanent magnet and preparation method thereof
By using pulse-charged coils and pneumatic vibrators to perform high-amplitude vibration and high-frequency pulse current orientation in sintered NdFeB magnetic powder, the problems of orientation damage and organic solvent residue in traditional processes are solved, and high efficiency and simplicity are achieved The preparation of sintered NdFeB rare earth permanent magnets in orientation improves the residual magnetic performance and production efficiency of the magnets.
Patent Information
- Application Number
- CN202411276337.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
AI Technical Summary
The orientation degree of sintered NdFeB permanent magnets in traditional powder metallurgy processes is easily damaged, and the prior art has problems such as complex process, low efficiency, and solvent residues affecting the performance of magnets when increasing the orientation degree by adding organic solvents.
The pulse-charged magnetic coil is used in combination with a pneumatic vibrator to apply high amplitude vibration and high frequency pulse current in both directions to orientation the magnetic powder, avoiding damage to the orientation in traditional pressure forming processes, and no need to add organic solvents, simplifying the production process.
A high-oriented sintered NdFeB rare earth permanent magnet is achieved, which improves residual magnetic performance, simplifies the production process, improves production efficiency, and overcomes the problems of orientation damage and solvent residue in traditional methods.
Smart Images

Figure BDA0005040295820000111 
Figure BDA0005040295820000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth permanent magnets, and in particular to a high-orientation sintered NdFeB rare earth permanent magnet and a preparation method thereof. Background Art
[0002] Sintered NdFeB permanent magnets are known as the "king of permanent magnets" for their excellent magnetic properties and are widely used in many fields such as computer disk drives, permanent magnet motors, precision instruments, and household appliances. High orientation of magnets is one of the key indicators for preparing high-performance sintered NdFeB magnets, which directly affects the key performance parameters of magnets such as remanence and magnetic energy product.
[0003] Sintered NdFeB permanent magnets are mainly prepared by powder metallurgy. This method includes multiple process steps such as batching, smelting, powder making, orientation pressing, and sintering. During the preparation process, magnetic field orientation technology is widely used to improve the orientation degree of the magnet, thereby improving its magnetic properties. The traditional powder metallurgy process has the problem of easy damage to the orientation degree during the orientation pressing process. In order to overcome this problem, researchers are constantly exploring new molding processes.
[0004] According to theoretical calculations in ferromagnetism, the remanent magnetic properties of polycrystalline NdFeB magnets are highly positively correlated with their orientation degree. Therefore, if the remanent magnetic properties of existing NdFeB magnets are to be improved, improving their orientation degree is a very direct and effective way. However, the current preparation process makes it difficult to prepare NdFeB magnetic materials with a higher orientation degree, especially in the powder sintering method, where it is difficult to achieve complete orientation of the raw powder of the magnet. The main reason is that during the orientation process of preparing NdFeB magnets by the existing powder sintering method, there is a large resistance between the magnetic powders, making it difficult for them to rotate completely freely along the direction of the orientation field. In addition, in the current traditional sintered NdFeB manufacturing process, the powder is pressed into a green body with a certain density, shape and size by simultaneously carrying out orientation pressing. During the pressing process of the powder into the green body, the oriented powder changes its orientation direction due to the pressing deformation, which in turn leads to problems such as damage to the orientation degree.
[0005] Chinese patents with publication numbers CN105931833A, CN115050564A and CN107393709A all use a wet molding process, that is, by adding some organic solvents to increase the fluidity of the powder and thereby improve the degree of orientation. However, this type of method still has disadvantages such as complex process, low efficiency, and solvent residue affecting the performance of the magnet.
[0006] The existing technology has the defects of easy orientation damage, long operation process, high energy consumption and low efficiency. Therefore, how to develop an efficient, simple, organic solvent-free and stable preparation method for sintered NdFeB permanent magnets has become a problem that needs to be solved urgently. Summary of the invention
[0007] In order to solve the above technical problems, the purpose of the present invention is to provide a high-orientation sintered NdFeB rare earth permanent magnet and a preparation method thereof, which can solve the problem of damaged orientation in the traditional orientation pressing process, while overcoming the defects caused by adding organic solvents to increase the orientation of the magnet in the prior art, simplifying the production process and improving production efficiency.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, the method comprising:
[0010] A mold filled with NdFeB magnetic powder is placed in a pulse magnetizing coil, and pneumatic vibrators are provided at both ends of the pulse magnetizing coil. Pulse current and pressureless vibration are applied to the pulse magnetizing coil to orient the magnetic powder to obtain oriented NdFeB magnetic powder, and high-orientation sintered NdFeB rare earth permanent magnets are obtained through post-processing.
[0011] The preparation method of the present invention reduces the friction between the magnetic powders and improves the fluidity between the magnetic powder particles by applying high-amplitude vibration in both directions at both ends of the magnetic powder, which is beneficial to the rotation of the magnetic powder particles during orientation; at the same time, a stronger orientation magnetic field is generated by high-frequency pulse current, making the orientation more complete and uniform. Compared with the traditional pressure forming process, the method of the present invention is conducive to obtaining a higher degree of orientation, solving the problem of damaged orientation degree in the traditional orientation pressing process. At the same time, no additives are added during the preparation method of the present invention, and no subsequent solvent removal operation is required. The defect of reducing the remanence of the magnet caused by incomplete removal of the organic solvent in the method of increasing the orientation degree of the magnet in the prior art by adding an organic solvent is overcome. The preparation method of the present invention simplifies the production process and improves production efficiency.
[0012] The "degree of orientation" in the present invention can be characterized by technical means such as XRD, and the "high degree of orientation" mentioned in the present invention is manifested as high remanence in macroscopic terms.
[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] Preferably, the median particle size of the NdFeB magnetic powder is 3.2-3.9 μm, for example, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm, 3.8 μm or 3.9 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the post-processing comprises cold isostatic pressing the highly oriented NdFeB magnetic powder to obtain a green compact.
[0016] It should be noted that the present invention does not specifically limit the specific composition of the NdFeB magnetic powder, which are all NdFeB magnetic powders commonly used in the art. For example, the NdFeB magnetic powder can be N series such as N50, N52, N54 or NH series such as N48H, N50H, N52H and other brands of magnetic powder.
[0017] Preferably, the cold isostatic pressing pressure is 150-250 MPa, for example, 150 MPa, 160 MPa, 170 MPa, 180 MPa, 190 MPa, 200 MPa, 210 MPa, 220 MPa, 230 MPa, 240 MPa or 250 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the holding time of the cold isostatic pressing is 1-2 minutes, for example, 1 minute, 1.5 minutes or 2 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the method further comprises sintering, performing primary heat treatment and secondary heat treatment on the green body in sequence under vacuum conditions to obtain a high-orientation sintered NdFeB rare earth permanent magnet.
[0020] Preferably, the vacuum degree of the vacuum condition is less than 3×10 -3 kPa.
[0021] Preferably, the sintering temperature is 1050-1080°C, for example, 1050°C, 1060°C, 1070°C or 1080°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] Preferably, the sintering time is 3-6 h, for example, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the temperature of the primary heat treatment is 880-920°C, for example, 880°C, 890°C, 900°C, 910°C or 920°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the time of the primary heat treatment is 2-5 h, for example, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the temperature of the secondary heat treatment is 480-520°C, for example, 480°C, 490°C, 500°C, 510°C or 520°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the time of the secondary heat treatment is 2-5 h, for example, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the vibration force of the pneumatic vibrator is 130-210N, for example, it can be 130N, 140N, 150N, 160N, 170N, 180N, 190N, 200N or 210N, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] In the present invention, the vibration force of the pneumatic vibrator is preferably 130-210N, and the vibration force can be adjusted by changing the air volume. The high-amplitude vibration applied in both directions at both ends of the magnetic powder can reduce the friction between the magnetic powders, improve the fluidity between the magnetic powder particles, and is conducive to the rotation of the magnetic powder particles during orientation; if the vibration force is too large, it will cause the oriented particles to return to a chaotic state, which is not conducive to the improvement of the orientation degree; if the vibration force is too small, the fluidity of the magnetic powder particles will be weakened, which is not conducive to the rotation of the particles.
[0029] Preferably, the output frequency of the charging magnetic power supply is 1 Hz-3 Hz, for example, 1 Hz, 2 Hz or 3 Hz, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the magnetic field of the pulse magnetization coil is 1.5-3T, for example, 1.5T, 2T, 2.5T or 3T, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the output voltage of the pulse magnetization coil is 2000-2500V, for example, it can be 2000V, 2100V, 2200V, 2300V, 2400V or 2500V, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] The output voltage of the pulse magnetization coil of the present invention is preferably 2000-2500V. The output voltage of the pulse magnetization coil affects the strength of the magnetic field. A high output voltage can obtain a high magnetic field strength, which is more conducive to the orientation distribution of magnetic powder particles. However, an excessively high output voltage places higher requirements on the equipment, increasing the difficulty. A low output voltage can reduce the magnetic field strength, thereby reducing the requirements on the equipment. However, a low magnetic field strength makes it difficult to completely orient the magnetic powder particles.
[0033] Preferably, the pulse current has a current magnitude of 7.0-9.0 kA, for example, 7.0 kA, 7.5 kA, 8.0 kA, 8.5 kA or 9.0 kA, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the orientation times are 5-20 times, for example, 5 times, 6 times, 7 times, 8 times, 9 times, 10 times, 11 times, 12 times, 13 times, 14 times, 15 times, 16 times, 17 times, 18 times, 19 times or 20 times, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] In the present invention, if the orientation times are too low, it is difficult to achieve complete orientation of the magnetic powder. When the orientation times are equal to or greater than 5 times, magnetic powder with a high degree of orientation can be obtained.
[0036] In a second aspect, the present invention provides a NdFeB rare earth permanent magnet, which is prepared according to the preparation method described in the first aspect.
[0037] The NdFeB rare earth permanent magnet provided by the present invention has a high degree of orientation, which greatly improves the remanence of the permanent magnet and achieves an improvement in coercive force.
[0038] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0039] Compared with the prior art, the present invention has at least the following beneficial effects:
[0040] The present invention uses high-frequency pulse current combined with pressureless vibration for orientation to obtain NdFeB magnetic powder with a high degree of orientation, and obtains a sintered NdFeB rare earth permanent magnet with a high degree of orientation through post-processing. The present invention applies high-amplitude vibration in both directions at both ends of the magnetic powder, which reduces the friction between the magnetic powders and improves the fluidity between the magnetic powder particles, which is beneficial to the rotation of the magnetic powder particles during orientation. At the same time, a stronger orientation magnetic field is generated by high-frequency pulse current, making the orientation more sufficient and uniform. Compared with the traditional pressure forming process, the method of the present invention is conducive to obtaining a higher degree of orientation; the preparation method of the present invention simplifies the production process and improves production efficiency. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is further described below by specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0042] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.
[0043] Example 1
[0044] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, the preparation method comprising the following steps:
[0045] A rubber mold filled with NdFeB magnetic powder is placed in a pulse magnetization coil with pneumatic vibrators at both ends, the vibration force of the pneumatic vibrator is 180N, and then a high-frequency pulse power supply is loaded to generate a pulse magnetic field for orientation. The orientation times are 10 times, and the magnetic field strength is 2.5T. After the orientation is completed, the vibration stops, and the NdFeB magnetic powder with a high degree of orientation is obtained;
[0046] The composition of the NdFeB magnetic powder is Nd 29.6 Fe 67.44 B 0.96 Co 1.5 Ga 0.1 Cu 0.15 Zr 0.25 , the median particle size is 3.9 μm;
[0047] The oriented rubber mold containing NdFeB magnetic powder is subjected to cold isostatic pressing at a pressure of 200 MPa for 60 seconds to obtain a green body;
[0048] The green body is placed in a vacuum of less than 3×10 -3 kPa, a temperature of 1065°C, vacuum sintering for 3.5 hours, a heating rate of 5°C / min, and air cooling to room temperature after sintering to obtain a sintered magnet;
[0049] The vacuum degree is less than 3×10 -3 kPa, temperature 900℃, primary heat treatment for 3h, heating rate 5℃ / min; after the heat treatment, air cooling to room temperature to obtain primary heat-treated magnet;
[0050] The primary heat treatment magnet is placed in a vacuum of less than 3×10 -3 kPa, temperature 500 ℃, secondary heat treatment for 3.5h, heating rate 5 ℃ / min; after the heat treatment, air cooling to room temperature to obtain high orientation sintered NdFeB rare earth permanent magnet.
[0051] Example 2
[0052] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, the preparation method comprising the following steps:
[0053] A rubber mold filled with NdFeB magnetic powder is placed in a pulse magnetization coil with pneumatic vibrators at both ends, the vibration force of the pneumatic vibrator is 130N, and then a high-frequency pulse power supply is loaded to generate a pulse magnetic field for orientation. The orientation times are 12 times, and the magnetic field strength is 3T. After the orientation is completed, the vibration stops, and the NdFeB magnetic powder with a high degree of orientation is obtained;
[0054] The composition of the NdFeB magnetic powder is Nd 29.3 Fe 68.04 B 0.96 Co 1.2 Ga 0.1 Cu 0.15 Zr 0.25 , the median particle size is 3.4 μm;
[0055] The oriented rubber mold containing NdFeB magnetic powder is subjected to cold isostatic pressing for 120 seconds at a pressure of 160 MPa to obtain a green body;
[0056] The green body is placed in a vacuum of less than 3×10 -3 kPa, a temperature of 1078°C, vacuum sintering for 3 h, a heating rate of 5°C / min, and air cooling to room temperature after sintering to obtain a sintered magnet;
[0057] The vacuum degree is less than 3×10 -3 kPa, temperature 890℃, primary heat treatment for 4h, heating rate 5℃ / min; after the heat treatment, air cooling to room temperature to obtain primary heat-treated magnet;
[0058] The primary heat treatment magnet is placed in a vacuum of less than 3×10 -3kPa, temperature 510 ℃ for 3h, heating rate 5 ℃ / min; after the heat treatment, air cooling to room temperature was carried out to obtain high orientation sintered NdFeB rare earth permanent magnet.
[0059] Example 3
[0060] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, the preparation method comprising the following steps:
[0061] A rubber mold filled with NdFeB magnetic powder is placed in a pulse magnetization coil with pneumatic vibrators at both ends, the vibration force of the pneumatic vibrator is 210N, and then a high-frequency pulse power supply is loaded to generate a pulse magnetic field for orientation. The orientation times are 5 times, and the magnetic field strength is 2.5T. After the orientation is completed, the vibration stops, and the NdFeB magnetic powder with a high degree of orientation is obtained;
[0062] The composition of the NdFeB magnetic powder is Nd 29.4 Fe 67.57 B 0.98 Co 1.5 Ga 0.1 Cu 0.15 Ti 0.3 , the median particle size is 3.65 μm;
[0063] The oriented rubber mold containing NdFeB magnetic powder is subjected to cold isostatic pressing at a pressure of 230 MPa for 40 seconds to obtain a green body;
[0064] The green body is placed in a vacuum of less than 3×10 -3 kPa, a temperature of 1080°C, vacuum sintering for 6 hours, a heating rate of 5°C / min, and air cooling to room temperature after sintering to obtain a sintered magnet;
[0065] The vacuum degree is less than 3×10 -3 kPa, temperature 920℃, primary heat treatment for 4h, heating rate 5℃ / min; after the heat treatment, air cooling to room temperature to obtain primary heat-treated magnet;
[0066] The primary heat treatment magnet is placed in a vacuum of less than 3×10 -3 kPa, temperature 480 ℃ secondary heat treatment for 3.5h, heating rate 5 ℃ / min; after the heat treatment, air cooling to room temperature to obtain high orientation sintered NdFeB rare earth permanent magnet.
[0067] Example 4
[0068] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, which is different from Embodiment 1 only in that, when preparing the high-orientation sintered NdFeB rare earth permanent magnet, the vibration force of the pneumatic vibrator is 100N.
[0069] Example 5
[0070] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet. The only difference from Embodiment 1 is that when preparing the high-orientation sintered NdFeB rare earth permanent magnet, the vibration force of the pneumatic vibrator is 250N.
[0071] Example 6
[0072] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, which is different from Embodiment 1 only in that, when preparing the high-orientation sintered NdFeB rare earth permanent magnet, the magnetic field strength is 1T.
[0073] Example 7
[0074] This embodiment provides a method for preparing a high-orientation sintered NdFeB rare earth permanent magnet, which is different from Embodiment 3 only in that the orientation times are 3 when preparing the high-orientation sintered NdFeB rare earth permanent magnet.
[0075] Comparative Example 1
[0076] This comparative example provides a sintered NdFeB rare earth permanent magnet, which is different from Example 1 only in that, when preparing the sintered NdFeB rare earth permanent magnet, the vibration force of the pneumatic vibrator is 0N, no high-frequency pulse power supply is loaded, and the magnetic field strength is 0T.
[0077] Comparative Example 2
[0078] This comparative example provides a sintered NdFeB rare earth permanent magnet, which is different from Example 1 only in that when preparing the sintered NdFeB rare earth permanent magnet, the vibration force of the pneumatic vibrator is 0N, a high-frequency pulse power supply is loaded, and the magnetic field strength is 2.5T.
[0079] Comparative Example 3
[0080] This comparative example provides a sintered NdFeB rare earth permanent magnet, which is different from Example 1 only in that, when preparing the sintered NdFeB rare earth permanent magnet, the vibration force of the pneumatic vibrator is 180N, no high-frequency pulse power supply is loaded, and the magnetic field strength is 0T.
[0081] Comparative Example 4
[0082] This comparative example provides a sintered NdFeB rare earth permanent magnet, which is prepared by oriented pressing. The specific method is as follows:
[0083] A mold filled with NdFeB magnetic powder is oriented and pressed in a magnetic field with a strength of 2.5T in a vertical pressing manner under argon protection to obtain a compact;
[0084] The green compact is subjected to cold isostatic pressing at a pressure of 200 MPa for 60 seconds to obtain a green compact;
[0085] The green body is placed in a vacuum of less than 3×10 -3 kPa, a temperature of 1065°C, vacuum sintering for 3.5 hours, a heating rate of 5°C / min, and air cooling to room temperature after sintering to obtain a sintered magnet;
[0086] The vacuum degree is less than 3×10 -3 kPa, temperature 900℃, primary heat treatment for 3h, heating rate 5℃ / min; after the heat treatment, air cooling to room temperature to obtain primary heat-treated magnet;
[0087] The primary heat treatment magnet is placed in a vacuum of less than 3×10 -3 kPa, temperature 500 ℃, secondary heat treatment for 3.5h, heating rate 5 ℃ / min; after the heat treatment, air cooling to room temperature to obtain sintered NdFeB rare earth permanent magnet.
[0088] Test method:
[0089] The sintered NdFeB rare earth permanent magnets obtained in Examples 1-7 and Comparative Examples 1-4 were tested, and the test results are shown in Table 1 below:
[0090] Table 1
[0091]
[0092]
[0093] The test results show that:
[0094] (1) It can be seen from Examples 1-3 that the present invention uses pulse current combined with pressureless vibration for orientation to obtain NdFeB magnetic powder with a high degree of orientation, and obtains a sintered NdFeB rare earth permanent magnet with a high degree of orientation after post-processing. The present invention applies high-amplitude vibration in both directions at both ends of the magnetic powder, reduces the friction between the magnetic powders, improves the fluidity between the magnetic powder particles, and is conducive to the rotation of the magnetic powder particles during orientation. At the same time, a stronger orientation magnetic field is generated by pulse current, making the orientation more sufficient and uniform. Compared with the traditional pressure forming process, the method of the present invention is conducive to obtaining a higher degree of orientation. The preparation method of the present invention simplifies the production process and improves production efficiency.
[0095] (2) By comparing Example 1 with Examples 4-5, it can be seen that the present invention further controls the vibration force of the pneumatic vibrator to be 130-210N. The high-amplitude vibration applied in both directions at both ends of the magnetic powder can reduce the friction between the magnetic powders, improve the fluidity between the magnetic powder particles, and facilitate the rotation of the magnetic powder particles during orientation; if the vibration force is too large, it will cause the oriented particles to return to a chaotic state, which is not conducive to the improvement of the orientation degree; if the vibration force is too small, the fluidity of the magnetic powder particles will be weakened, which is not conducive to the rotation of the particles.
[0096] (3) By comparing Example 1 with Example 6, it can be seen that the present invention further controls the magnetic field size of the pulse magnetization coil to 1.5-3T. Since the magnetic field size of the pulse magnetization coil is determined by the output voltage of the pulse magnetization coil; a low magnetic field strength requires a lower output voltage of the pulse magnetization coil, thereby reducing the requirements for the equipment. However, it is difficult to achieve complete orientation of the magnetic powder particles at a low magnetic field strength. The higher the magnetic field strength, the more conducive it is to the oriented distribution of the magnetic powder particles. However, an excessively high output voltage places higher requirements on the equipment, increasing the difficulty and cost of preparation.
[0097] (4) By comparing Example 3 with Example 7, it can be seen that the present invention further controls the number of orientations to be between 5 and 20 times. When the number of orientations is equal to or greater than 5 times, high-orientation magnetic powder can be obtained. If the number of orientations is too small, it is not conducive to achieving a high degree of orientation of the magnetic powder.
[0098] (5) It can be seen from Example 1 and Comparative Example 1 that the present invention obtains NdFeB magnetic powder with high orientation by combining high-frequency pulse current with pressureless vibration, and obtains high-orientation sintered NdFeB rare earth permanent magnet after post-treatment. However, when no pneumatic vibrator is used, that is, the vibration force is 0N, and no high-frequency pulse power supply is loaded, that is, the magnetic field strength is 0T, it is impossible to improve the orientation degree of NdFeB magnetic powder, and the permanent magnet obtained after sintering has very low remanence.
[0099] (6) It can be seen from Example 1 and Comparative Example 2 that the present invention obtains NdFeB magnetic powder with a high orientation degree by orienting through high-frequency pulse current combined with pressureless vibration, and obtains a sintered NdFeB rare earth permanent magnet with a high orientation degree after post-treatment. However, when the pneumatic vibrator is not used, that is, the vibration force is 0N, the orientation degree of the NdFeB magnetic powder cannot be improved due to the large friction between the magnetic powders, and the remanence of the permanent magnet obtained after sintering is not significantly improved.
[0100] (7) It can be seen from Example 1 and Comparative Example 3 that the present invention obtains NdFeB magnetic powder with a high orientation degree by orienting through high-frequency pulse current combined with pressureless vibration, and obtains a high-orientation sintered NdFeB rare earth permanent magnet after post-treatment. When no high-frequency pulse power supply is loaded, that is, when the magnetic field strength is 0T, it is impossible to improve the orientation degree of the NdFeB magnetic powder, and the permanent magnet obtained after sintering has a very low remanence.
[0101] (8) It can be seen from Example 1 and Comparative Example 4 that when the orientation pressing method is adopted, it is impossible to further improve the orientation degree of NdFeB magnetic powder, and the remanence of the permanent magnet obtained after sintering is significantly reduced.
[0102] In summary, the present invention reduces the friction between magnetic powders and improves the fluidity between magnetic powder particles by applying high-amplitude vibration in both directions at both ends of the magnetic powder, which is beneficial to the rotation of magnetic powder particles during orientation; at the same time, a stronger orientation magnetic field is generated by pulse current, making the orientation more sufficient and uniform. By using pulse current combined with pressureless vibration to obtain high-orientation NdFeB magnetic powder, and obtaining high-orientation sintered NdFeB rare earth permanent magnets after post-processing, the preparation method of the present invention simplifies the production process and improves production efficiency.
[0103] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a highly oriented sintered NdFeB rare earth permanent magnet. It is characterized in that The method comprises: A mold filled with NdFeB magnetic powder is placed in a pulse magnetizing coil, and pneumatic vibrators are provided at both ends of the pulse magnetizing coil. Pulse current and pressureless vibration are applied to the pulse magnetizing coil to orient the magnetic powder to obtain oriented NdFeB magnetic powder, and high-orientation sintered NdFeB rare earth permanent magnets are obtained through post-processing.
2. The preparation method according to claim 1, It is characterized in that The median particle size of the NdFeB magnetic powder is 3.2-3.9 μm; Preferably, the post-processing comprises cold isostatic pressing the oriented NdFeB magnetic powder to obtain a green compact.
3. The preparation method according to claim 2, It is characterized in that The cold isostatic pressing pressure is 150-250 MPa; Preferably, the holding time of the cold isostatic pressing is 1-2 minutes.
4. The preparation method according to claim 2 or 3, It is characterized in that The method further comprises sequentially sintering, performing primary heat treatment and secondary heat treatment on the green body under vacuum conditions to obtain a high-orientation sintered NdFeB rare earth permanent magnet.
5. The preparation method according to claim 4, It is characterized in that The vacuum degree of the vacuum condition is less than 3×10 - 3 kPa; Preferably, the sintering temperature is 1050-1080°C; Preferably, the sintering time is 3-6 hours.
6. The preparation method according to claim 4 or 5, It is characterized in that The temperature of the primary heat treatment is 880-920°C; Preferably, the primary heat treatment lasts for 2-5 hours.
7. The preparation method according to any one of claims 4 to 6, It is characterized in that The temperature of the secondary heat treatment is 480-520°C; Preferably, the secondary heat treatment lasts for 2-5 hours.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The vibration force of the pneumatic vibrator is 130-210N.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that The output frequency of the pulse magnetization power supply is 1Hz-3Hz; Preferably, the magnetic field of the pulse magnetization coil is 1.5-3T; Preferably, the output voltage of the pulse magnetization coil is 2000-2500V; Preferably, the current magnitude of the pulse current is 7.0-9.0 kA; Preferably, the orientation times are 5-20 times.
10. A neodymium iron boron rare earth permanent magnet, It is characterized in that The NdFeB rare earth permanent magnet is prepared according to the preparation method according to any one of claims 1-9.
Citation Information
Cited By
A directional sintering process of anisotropic permanent magnetic material
CN122762466A