Method for improving surface flatness of silicon wafer and solar cell silicon wafer manufactured by same
By laser etching and multi-step processing on the surface of the silicon wafer before alkali spreading, the problem of difficult removal of wire marks on the surface of the silicon wafer is solved, and the high flatness and reflectivity are improved, which reduces production costs and complexity are avoided. Impact on other performance.
Patent Information
- Application Number
- CN202411083386.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively eliminate line marks on the surface of silicon wafers after alkali casting, affecting surface flatness and reflectivity, and changing the alkali casting process conditions may affect other performances, increasing production costs and complexity.
Use laser etching to form grooves before alkali spreading, and through multiple steps, including water washing, oxidation reaction, pickling and drying, combining different concentrations of alkali and additives, remove line marks and damage layers, and generate high flatness and Reflectivity silicon wafer.
Without changing the alkali-throwing process conditions, effectively eliminate the wire marks on the surface of the silicon wafer, improve the surface flatness and reflectivity, reduce production costs and complexity, and avoid the impact on other performance.
Smart Images

Figure CN119008383A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and more specifically to a method for improving the surface flatness of a silicon wafer and a solar cell silicon wafer manufactured using the method. Background Art
[0002] Solar cells are semiconductor devices that convert sunlight directly into electrical energy. As they are green and environmentally friendly products that do not cause environmental pollution and utilize renewable resources, solar cells have broad development prospects in today's energy shortage situation.
[0003] In the field of semiconductor material processing technology, silicon wafers are the basic semiconductor materials, and their surface quality directly affects the subsequent semiconductor device process and device performance. In the silicon wafer manufacturing process, alkali polishing is a common surface treatment method, which can effectively remove the mechanical damage layer on the surface of the silicon wafer and improve the surface flatness and reflectivity of the silicon wafer. However, the surface of the silicon wafer after direct alkali polishing often leaves obvious line marks, which will affect the appearance of the silicon wafer and the subsequent doping effect.
[0004] In the prior art, the line marks after alkali polishing are mainly reduced by changing the process conditions of alkali polishing, such as temperature, time, concentration, etc. In addition, there are some technologies that improve the surface quality of silicon wafers by performing additional grinding and polishing on silicon wafers after alkali polishing, but changing the process conditions of alkali polishing may affect other properties of silicon wafers, such as resistivity, lattice structure, etc. Secondly, additional grinding and polishing processes will increase production costs and complexity.
[0005] Therefore, how to effectively eliminate the line marks on the surface of silicon wafers and improve the surface flatness and reflectivity of silicon wafers without changing the alkali polishing process conditions is an urgent problem that needs to be solved in current silicon wafer manufacturing technology. Summary of the invention
[0006] The content of this application is used to introduce concepts in a brief form, which will be described in detail in the detailed implementation section below. The content of this application is not intended to identify the key features or essential features of the technical solution claimed for protection, nor is it intended to limit the scope of the technical solution claimed for protection.
[0007] Some embodiments of the present application propose a method for improving the surface flatness of a silicon wafer and a solar cell silicon wafer manufactured therefrom to solve the technical problems mentioned in the above background technology section.
[0008] As a first aspect of the present application, some embodiments of the present application provide a method for improving the surface flatness of a silicon wafer, comprising: alkaline polishing the silicon wafer; washing the silicon wafer with water and placing it in an ozone tank for an oxidation reaction; acid-washing and rinsing the silicon wafer and then drying it; the method for improving the surface flatness of the silicon wafer also includes: before alkaline polishing the silicon wafer, using a laser to etch the surface of the silicon wafer so that the etched surface of the silicon wafer forms grooves arranged in sequence.
[0009] Furthermore, the opening width of the groove is in a range of 10 micrometers to 15 micrometers, and the groove is in a "V" shape or a semicircular shape.
[0010] Furthermore, the wavelength of the laser used for laser etching is 1064 nanometers, the power is 4-5W, the frequency is 20kHz, and the pulse width is 10ns.
[0011] Furthermore, between using laser to etch the surface of the silicon wafer and alkaline polishing the silicon wafer, the process also includes: immersing the laser-etched silicon wafer in a cleaning solution for pre-cleaning to remove organic dirt on the surface of the silicon wafer; and rinsing the pre-cleaned silicon wafer in a deionized water tank to remove impurities desorbed from the surface and residual chemicals.
[0012] Furthermore, the method of alkali polishing of silicon wafers comprises: placing the washed silicon wafer into a tank containing a first alkali solution for reaction, removing the laser etching layer and part of the line marks, and preliminarily preparing a tower base of appropriate size on the surface of the silicon wafer; wherein the first alkali solution comprises NaOH or KOH with a mass percentage concentration of 5%-10%, the alkali polishing temperature is 75-80°C, and the reaction time is 100-200s.
[0013] Furthermore, between the step of alkali polishing the silicon wafer and the step of washing the silicon wafer with water and then placing it in an ozone tank for oxidation reaction, the method further includes: placing the silicon wafer with a preliminary growth of a suitable tower base into a tank containing a second alkali solution and hydrogen peroxide, micro-etching the surface of the silicon wafer, and removing the by-products remaining on the surface of the silicon wafer; wherein the second alkali solution comprises NaOH or KOH with a mass percentage concentration of 2.1%-3.0% and hydrogen peroxide with a mass percentage ratio of 1% to 10%, the alkali solution temperature is 50-70°C, and the reaction time is 40-100s.
[0014] Furthermore, the method of washing the silicon wafer and then placing it in an ozone tank for oxidation reaction comprises: placing the silicon wafer in a deionized water tank for rinsing to remove impurities and residual chemicals desorbed from the surface; placing the washed silicon wafer in a tank containing a third alkali solution and a polishing additive for reaction to remove the last damaged layer on the surface of the silicon wafer, eliminate line marks, and obtain a silicon wafer with high surface flatness and reflectivity; wherein the third alkali solution includes NaOH or KOH with a mass percentage concentration of 5%-10%, and the volume percentage of the additive is 1 % to 2%, its main components are water, sodium benzoate, defoaming agent and surfactant, the reaction temperature is 75-80℃, the reaction time is 100-200s; then the silicon wafer is placed in a deionized water tank for rinsing to remove impurities and residual chemicals desorbed from the surface; the silicon wafer with the tower base grown is placed in an ozone tank to oxidize and remove the additives remaining on the surface of the silicon wafer, and at the same time generate an oxide layer; wherein the ozone liquid includes hydrochloric acid with a mass percentage concentration of 0.10%-0.15%, and the rest is deionized water, and the ozone concentration is 20-60ppm.
[0015] Furthermore, the method of drying the silicon wafer after pickling and rinsing includes: soaking the oxidized silicon wafer in a pickling tank containing hydrofluoric acid to peel off the oxide layer; rinsing the silicon wafer after hydrofluoric acid etching in a slow pulling tank; and drying the rinsed silicon wafer in a drying tank.
[0016] Furthermore, the silicon wafer is placed in the slow pull tank for rinsing for 30 to 60 seconds, the reaction temperature is 20-30°C, the drying time is 500-800 seconds, and the drying temperature is 80-90°C.
[0017] As a second aspect of the present application, some embodiments of the present application provide a solar cell silicon wafer, which is manufactured by the above-mentioned method for improving the surface flatness of a silicon wafer.
[0018] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0019] The present invention uses a laser to etch the surface of the silicon wafer before alkali polishing the silicon wafer, thereby effectively eliminating line marks on the surface of the silicon wafer without changing the alkali polishing process conditions, improving the surface flatness and reflectivity of the silicon wafer, and also avoiding the impact on other properties of the silicon wafer (such as resistivity, lattice structure, etc.) caused by changing the alkali polishing process conditions, reducing additional grinding and polishing processes, and reducing production costs and complexity. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings constituting a part of this application are used to provide a further understanding of this application, so that other features, purposes and advantages of this application become more obvious. The illustrative embodiment drawings and their descriptions of this application are used to explain this application and do not constitute an improper limitation on this application.
[0021] In addition, throughout the drawings, the same or similar reference numerals represent the same or similar elements. It should be understood that the drawings are schematic and that the components and elements are not necessarily drawn to scale.
[0022] Figure 1 is a step diagram of a method for improving the surface flatness of a silicon wafer according to an embodiment of the present application;
[0023] Figure 2 It is a schematic diagram of a groove formed by etching a silicon wafer by laser in a method for improving the surface flatness of a silicon wafer according to an embodiment of the present application;
[0024] Figure 3 This is a comparison diagram of the silicon wafer surface obtained before laser etching treatment (A) and after laser treatment (B) and alkali polishing in a method for improving the surface flatness of a silicon wafer according to an embodiment of the present application. DETAILED DESCRIPTION
[0025] Embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although certain embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present disclosure. It should be understood that the drawings and embodiments of the present disclosure are only for exemplary purposes and are not intended to limit the scope of protection of the present disclosure.
[0026] It should also be noted that, for ease of description, only the parts related to the invention are shown in the drawings. In the absence of conflict, the embodiments and features in the embodiments of the present disclosure can be combined with each other.
[0027] It should be noted that the concepts such as "first" and "second" mentioned in the present disclosure are only used to distinguish different devices, modules or units, and are not used to limit the order or interdependence of the functions performed by these devices, modules or units.
[0028] It should be noted that the modifications of "one" and "plurality" mentioned in the present disclosure are illustrative rather than restrictive, and those skilled in the art should understand that unless otherwise clearly indicated in the context, it should be understood as "one or more".
[0029] The names of the messages or information exchanged between multiple devices in the embodiments of the present disclosure are only used for illustrative purposes and are not used to limit the scope of these messages or information.
[0030] The present disclosure will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0031] like Figures 1 to 3As shown, some embodiments of an embodiment of the present application provide a method for improving the surface flatness of a silicon wafer, including: alkaline polishing of the silicon wafer; water washing the silicon wafer and then placing it in an ozone tank for oxidation reaction; acid cleaning and rinsing the silicon wafer and then drying it; the method for improving the surface flatness of the silicon wafer also includes: before alkaline polishing of the silicon wafer, using a laser to etch the surface of the silicon wafer so that the surface of the etched silicon wafer forms grooves arranged in sequence, and the opening width range of the grooves is 10 microns to 15 microns, where the opening width range of the grooves depends on parameters such as the laser spot size and power.
[0032] Specifically, before alkali polishing the silicon wafer, the surface of the silicon wafer is etched with a laser so that grooves are arranged in sequence on the surface of the etched silicon wafer. The laser used for laser etching here is a Nd:YAG laser with a wavelength of 1064 nanometers. The laser power is set to 4-5W, the frequency is 20kHz, and the pulse width is 10ns. Place the original silicon wafer under the laser, adjust the distance between the laser head and the silicon wafer to 1-2mm, and then turn on the laser to perform laser etching on the silicon wafer. During this process, the laser will automatically scan according to the preset parameters to ensure that every part of the silicon wafer surface can be evenly etched. Figure 2 As shown, the groove is in a "V" shape, and the shape of the opening of the groove is related to the laser process, and can also be a semicircular pit-shaped opening with a width of 10 to 15 microns.
[0033] Since laser etching is a precise and efficient processing method, it can accurately control the etching depth and accuracy of the silicon wafer surface, thereby improving the surface flatness and reflectivity of the silicon wafer, providing a good foundation for the subsequent alkaline polishing process, and can reduce the concentration of the subsequent alkaline polishing solution within a certain range, thereby reducing production costs.
[0034] In a specific embodiment, a pre-cleaning and water washing step is included between using a laser to etch the surface of a silicon wafer and alkaline polishing the silicon wafer: the silicon wafer after laser etching is immersed in a cleaning solution for pre-cleaning to remove organic dirt on the surface of the silicon wafer; the silicon wafer after pre-cleaning is placed in a deionized water tank for rinsing to remove impurities desorbed from the surface and residual chemicals.
[0035] Specifically, the cleaning solution used in the pre-cleaning step includes HF with a mass percentage concentration of 2.0%-3.0% and HCl with a mass percentage of 1%-8%, and the immersion treatment time is 40-100s. The silicon wafer after pre-cleaning is placed in a deionized water tank for rinsing, and the rinsing time is 100-200s. The chemicals and organic dirt remaining on the surface of the silicon wafer treated by the pre-cleaning and water washing steps are removed, providing better reaction conditions for the next step of alkaline polishing.
[0036] More specifically, the step of alkali polishing the silicon wafer includes: placing the silicon wafer after the above-mentioned water washing step into a tank containing a first alkali solution for reaction, removing the laser etching layer and part of the line marks, and preliminarily preparing a tower base of appropriate size on the surface of the silicon wafer, where the tower base refers to a square pyramid tower base, and the size of the tower base is proportional to the reaction intensity (reaction time, temperature, alkali solution concentration); wherein the first alkali solution includes NaOH or KOH with a mass percentage concentration of 5%-10%, the alkali polishing temperature is 75-80°C, and the reaction time is 100-200s.
[0037] Since the silicon wafer is laser etched and pre-cleaned before alkaline polishing, the surface of the silicon wafer has been preliminarily processed at this time. Therefore, the concentration of the first alkaline solution required for alkaline polishing and thinning the silicon wafer, as well as the temperature and time required for the reaction are reduced accordingly, thereby reducing production costs.
[0038] In a specific embodiment, after washing the silicon wafer, placing it in an ozone tank for oxidation reaction and alkali polishing the silicon wafer also include: placing the silicon wafer with a suitable tower base initially grown in a tank containing a second alkali solution and hydrogen peroxide, micro-etching the surface of the silicon wafer, the hydrogen peroxide plays the role of oxidation byproducts (dirt), on this basis, the second alkali solution removes the dirt after oxidation through micro-etching, effectively removing the byproducts remaining on the surface of the silicon wafer, the byproduct referred to here is sodium silicate generated by the reaction of silicon and alkali, and further cleaning the surface of the silicon wafer. Wherein, the second alkali solution includes NaOH or KOH with a mass percentage concentration of 2.1%-3.0%, and hydrogen peroxide with a mass percentage of 1%-10%, the alkali solution temperature is 50-70°C, and the reaction time is 40-100s.
[0039] The method of washing a silicon wafer and placing it in an ozone tank for oxidation reaction comprises: placing the silicon wafer in a deionized water tank for rinsing to remove impurities and residual chemicals desorbed from the surface; placing the washed silicon wafer in a tank containing a third alkali solution and a polishing additive for reaction to remove the last damaged layer on the surface of the silicon wafer, eliminate line marks, and obtain a silicon wafer with high surface flatness and reflectivity. Wherein, the third alkali solution includes NaOH or KOH with a mass percentage concentration of 5%-10%, the volume percentage of the additive is 1%-2%, and its main components are water, sodium benzoate, defoamer and surfactant, the reaction temperature is 75-80°C, and the reaction time is 100-200s. Then, the silicon wafer is placed in a deionized water tank for rinsing to remove impurities and residual chemicals that have not been desorbed from the surface. The impurities refer to sodium silicate generated by the reaction of silicon and alkali, which is the same substance as the by-product mentioned above. Sodium silicate is viscous, and some sodium silicate will adhere to the surface of the silicon wafer; the residual chemicals are organic matter in the additive. The rinsing time here is 80-150s. The silicon wafer with the tower base is placed in an ozone tank to oxidize and remove the additives remaining on the surface of the silicon wafer, and at the same time, an oxide layer is generated; wherein the ozone liquid includes hydrochloric acid with a mass percentage concentration of 0.10%-0.15%, and the rest is deionized water, and the ozone concentration is 20-60ppm.
[0040] like Figure 3 As shown, by performing laser etching and secondary alkali polishing on the surface of the original silicon wafer, the damaged layer on the surface of the original silicon wafer is etched away, and the flatness and reflectivity of the silicon wafer surface after alkali polishing can be improved (the reflectivity is greater than 42%). The use of laser etching on the surface of the silicon wafer greatly increases the looseness and roughness of the silicon wafer surface, so that the alkali polishing process can remove the damaged layer more evenly, and can effectively eliminate the line marks on the surface of the silicon wafer, and will not change the process conditions of alkali polishing, thereby avoiding possible effects on other properties of the silicon wafer. Compared with the grinding and polishing treatment in the prior art, it can not only reduce production costs and complexity, but also more effectively improve the flatness and reflectivity of the silicon wafer surface. At the same time, since the line marks on the surface of the silicon wafer are effectively eliminated, the silicon wafer has a more uniform process effect in the subsequent semiconductor device manufacturing process, thereby improving the performance and reliability of the semiconductor device, and has broad market application prospects.
[0041] In a specific embodiment, the method of drying the silicon wafer after pickling and rinsing comprises soaking the oxidized silicon wafer in a pickling tank containing hydrofluoric acid to peel off the oxide layer. The silicon wafer after hydrofluoric acid etching is placed in a slow pull tank for rinsing; the rinsed silicon wafer is placed in a drying tank for drying. The mass percentage concentration of the hydrofluoric acid solution referred to here is 4.0% to 6.0%. The pickling time is 200-300s. The slow pull rinsing time is 30-60s, the temperature is 20-30°C, and the slow pull speed of the robotic arm above the tank is 5mm / s to remove water stains on the surface of the silicon wafer. The drying time is 500-800s, and the temperature is 80-90°C.
[0042] In summary, in a specific embodiment, the method for improving the surface flatness of a silicon wafer should include the following steps:
[0043] S100, using laser to etch the surface of the silicon wafer so that grooves arranged in sequence are formed on the surface of the etched silicon wafer.
[0044] S200, immersing the laser-etched silicon wafer in a cleaning solution for pre-cleaning.
[0045] S300, placing the pre-cleaned silicon wafer into a deionized water tank for rinsing.
[0046] S400, placing the washed silicon wafer into a tank containing the first alkaline solution for reaction, removing the laser etching layer and part of the line marks, and preliminarily preparing a tower base of appropriate size on the surface of the silicon wafer.
[0047] S500, placing the silicon wafer with the appropriate tower base initially grown thereon into a tank containing a second alkali solution and hydrogen peroxide, micro-etching the surface of the silicon wafer to remove the byproducts remaining on the surface of the silicon wafer.
[0048] S600, rinse the silicon wafer in a deionized water tank.
[0049] S700, placing the washed silicon wafer into a tank containing a third alkali solution and a polishing additive for reaction, removing the last damaged layer on the surface of the silicon wafer and eliminating line marks.
[0050] S800, rinse the silicon wafer in a deionized water tank.
[0051] S900, put the silicon wafer with the tower base into the ozone tank to oxidize and remove the additives remaining on the surface of the silicon wafer, and at the same time generate an oxide layer.
[0052] S1000, soak the oxidized silicon wafer in a pickling tank containing hydrofluoric acid to peel off the oxide layer.
[0053] S1100, placing the silicon wafer after hydrofluoric acid etching in a slow pull tank for rinsing.
[0054] S1200, placing the rinsed silicon wafer into a drying tank for drying.
[0055] Specifically, in a specific embodiment, a solar cell silicon wafer is manufactured using the above method steps S100 to S1200.
[0056] The above descriptions are only some preferred embodiments of the present disclosure and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the embodiments of the present disclosure is not limited to the technical solutions formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the above-mentioned inventive concept. For example, the above-mentioned features are replaced with the technical features with similar functions disclosed in the embodiments of the present disclosure (but not limited to) and the technical solutions formed.
Claims
1. A method for improving the surface flatness of a silicon wafer, comprising: Alkaline polishing of silicon wafers; After washing the silicon wafer, place it in an ozone tank for oxidation reaction; Drying the silicon wafer after pickling and rinsing; Features: The method for improving the surface flatness of the silicon wafer also includes: Before alkaline polishing of the silicon wafer, the surface of the silicon wafer is etched with a laser so that grooves arranged in sequence are formed on the surface of the etched silicon wafer.
2. The method for improving the surface flatness of a silicon wafer according to claim 1, characterized in that: The opening width of the groove is in the range of 10 microns to 15 microns, and the groove is in a "V" shape or a semicircular shape.
3. The method for improving the surface flatness of a silicon wafer according to claim 1 or 2, characterized in that: The laser used for the laser etching has a wavelength of 1064 nanometers, a power of 4-5 W, a frequency of 20 kHz, and a pulse width of 10 ns.
4. The method for improving the surface flatness of a silicon wafer according to claim 1, characterized in that: Between using laser to etch the surface of silicon wafer and alkali polishing of silicon wafer, it also includes: The laser-etched silicon wafer is immersed in a cleaning solution for pre-cleaning to remove organic dirt on the surface of the silicon wafer; The pre-cleaned silicon wafer is rinsed in a deionized water tank to remove impurities and residual chemicals desorbed from the surface.
5. The method for improving the surface flatness of a silicon wafer according to claim 4, characterized in that: The method for alkali polishing of silicon wafers comprises: The washed silicon wafer is placed in a tank containing the first alkali solution for reaction, the laser etching layer and part of the line marks are removed, and a tower base of appropriate size is preliminarily prepared on the surface of the silicon wafer; Wherein, the first alkali solution comprises NaOH or KOH with a mass percentage concentration of 5%-10%, the alkali polishing temperature is 75-80°C, and the reaction time is 100-200s.
6. The method for improving the surface flatness of a silicon wafer according to claim 5, characterized in that: The step of alkali polishing the silicon wafer and the step of washing the silicon wafer with water and then placing it in an ozone tank for oxidation reaction also includes: The silicon wafer with the appropriate tower base initially grown thereon is placed in a tank containing the second alkali solution and hydrogen peroxide, and the surface of the silicon wafer is micro-etched to remove the byproducts remaining on the surface of the silicon wafer; The second alkali solution comprises NaOH or KOH with a mass percentage concentration of 2.1%-3.0% and hydrogen peroxide with a mass percentage of 1%-10%, the alkali solution temperature is 50-70° C., and the reaction time is 40-100s.
7. The method for improving the surface flatness of a silicon wafer according to claim 6, characterized in that: The method of washing the silicon wafer with water and then placing it in an ozone tank for oxidation reaction comprises: Rinse the silicon wafer in a deionized water tank to remove impurities and residual chemicals desorbed from the surface; The washed silicon wafer is placed in a tank containing a third alkali solution and a polishing additive to react, thereby removing the last damaged layer on the surface of the silicon wafer and eliminating the line marks, thereby obtaining a silicon wafer with high surface flatness and reflectivity; The third alkali solution comprises NaOH or KOH with a mass percentage concentration of 5%-10%, the volume percentage of the additive is 1%-2%, and its main components are water, sodium benzoate, defoamer and surfactant, the reaction temperature is 75-80°C, and the reaction time is 100-200s; The silicon wafer is then rinsed in a deionized water tank to remove impurities and residual chemicals desorbed from the surface; The silicon wafer with the tower base is placed in an ozone tank to oxidize and remove the additives remaining on the surface of the silicon wafer, while forming an oxide layer; The ozone liquid includes hydrochloric acid with a mass percentage concentration of 0.10%-0.15%, and the rest is deionized water, and the ozone concentration is 20-60ppm.
8. The method for improving the surface flatness of a silicon wafer according to claim 7, characterized in that: The method for drying the silicon wafer after pickling and rinsing comprises: The oxidized silicon wafer is immersed in a pickling tank containing hydrofluoric acid to peel off the oxide layer; The silicon wafer after hydrofluoric acid etching is placed in a slow pull tank for rinsing; The rinsed silicon wafers are placed in a drying tank for drying.
9. The method for improving the surface flatness of a silicon wafer according to claim 8, characterized in that: The silicon wafer is placed in the slow pull tank for rinsing for 30 to 60 seconds, the reaction temperature is 20-30°C, the drying time is 500-800 seconds, and the drying temperature is 80-90°C.
10. A solar cell silicon wafer, characterized in that: The method for improving the surface flatness of a silicon wafer is used to make the silicon wafer.
Citation Information
Cited By
Secondary alkali polishing process of TOPCon solar cell
CN120435093A