Method for preparing wafer-level Bi2O2Se / HfO2 thin film transistor through full magnetron sputtering

Bi2O2Se and HfO2 films were prepared by full magnetron sputtering technology and Ni electrodes were formed on them, which solved the problems of poor film matching and negative threshold voltage in the prior art, and achieved high-performance transistor preparation, showing positive threshold value Voltage and high current switching ratio.

CN119008410APending Publication Date: 2024-11-22NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066367.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the matching performance of Bi2O2Se and HfO2 films is poor, resulting in a problem that the current switch is low and the threshold voltage is negative.

Method used

The wafer-level Bi2O2Se/HfO2 film is prepared by the full magnetron sputtering method. Bi2O2Se and HfO2 films are deposited on the substrate through magnetron sputtering technology, and Ni films are formed on it as source electrode, drain electrode and gate electrode to ensure that Good matching between films.

Benefits of technology

Good adaptability between films is achieved, and transistors with positive threshold voltage are prepared, with current switching ratio greater than 105, and excellent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008410A_ABST
    Figure CN119008410A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductor films and devices, and discloses a method for preparing a wafer-level Bi2O2Se / HfO2 thin film transistor through full magnetron sputtering. The preparation method comprises the following specific steps: depositing a layer of Bi2O2Se film on a sapphire substrate by using a magnetron sputtering technology, preparing a Bi2O2Se channel array by using a technology of combining ultraviolet lithography and reactive ion etching, preparing an HfO2 dielectric layer by using the magnetron sputtering technology, and preparing an electrode by using the technology of combining ultraviolet lithography and magnetron sputtering. By adopting the method, a device with excellent performance can be prepared in a large area, and compared with a traditional preparation process, the wafer-level Bi2O2Se / HfO2 thin film transistor prepared by utilizing magnetron sputtering has the advantages that the matching performance among all layers of thin films is good, the performance is excellent, and the threshold voltage is positive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor thin films and devices, and specifically relates to a method for preparing wafer-level Bi 2 O 2 Se / HfO 2 Thin film transistor method. Background Art

[0002] Quasi-two-dimensional layered Bi 2 O 2 Se semiconductors have the advantages of high electron mobility, suitable band gap, and good environmental stability, and are considered to be ideal channel materials for the next generation of high-speed and low-energy information processing chips. 2 With the advantages of high dielectric constant, good thermal stability and chemical stability, it is considered to be an important dielectric material for the next generation of high-performance field effect transistor devices. 2 O 2 The main preparation method of Se is chemical vapor deposition, HfO 2 The main method for preparing dielectric layers is atomic layer deposition. However, both methods have similarities with Bi 2 O 2 The Se film has poor matching, low current switching, and negative threshold voltage. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing wafer-level Bi 2 O 2 Se / HfO 2 A method for thin film transistors is provided, thereby preparing transistors with good film matching, excellent performance and positive threshold voltage.

[0004] The present invention provides a method for preparing wafer-level Bi by full magnetron sputtering 2 O 2 Se / HfO 2 A method for a thin film transistor, comprising the following steps:

[0005] Step 1: Bi 2 O 2 Se target was used as the target material and magnetron sputtering was performed on a clean substrate to prepare Bi 2 O 2 Se thin film;

[0006] Step 2: Bi prepared in step 1 2 O 2 UV lithography is used on the Se film to define the channel pattern, and Ar ion etching or reactive ion etching is used to remove the excess film to form the Bi 2 O 2Se channel array;

[0007] Step 3: Magnetron sputtering technology is used to deposit Bi 2 O 2 A Ni film is deposited on the Se channel array as source and drain electrodes;

[0008] Step 4: Preparation of HfO by magnetron sputtering technology 2 The film serves as a gate dielectric layer;

[0009] Step 5: Deposit a Ni film on the gate dielectric layer as a gate electrode using magnetron sputtering technology.

[0010] Preferably, in step 1, Bi 2 O 2 The thickness of the Se film is 4-10 nm, and the magnetron sputtering temperature is 400-600°C.

[0011] Preferably, in step 4, HfO 2 The film thickness is 15-60nm, the magnetron sputtering temperature is room temperature, and the HfO 2 HfO was prepared as a target material using magnetron sputtering technology 2 film.

[0012] Preferably, in step 3 and step 5, the thickness of the Ni film is 10-100 nm, the magnetron sputtering temperature is room temperature, and the Ni film is deposited by magnetron sputtering technology using Ni as a target material.

[0013] Compared with the prior art, the present invention can produce devices with uniform film thickness over a large area, and the prepared transistor films have good compatibility, which enables the transistor to exhibit excellent performance such as positive threshold voltage and higher current switching ratio.

[0014] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The Bi prepared on the sapphire substrate in Example 1 of the present invention 2 O 2 Raman spectrum characterization picture of Se film;

[0016] Figure 2 The optical photograph and device optical micrograph of a large-area transistor array prepared on a sapphire substrate in Example 1 of the present invention;

[0017] Figure 3 The transfer characteristic curve of the transistor prepared in Example 1 of the present invention;

[0018] Figure 4The transfer characteristic curve of the transistor prepared in Example 2 of the present invention;

[0019] Figure 5 The transfer characteristic curve of the transistor prepared in Example 3 of the present invention, Figure a is Ag, and Figure b is Cu. DETAILED DESCRIPTION

[0020] The present invention adopts magnetron sputtering technology to prepare HfO 2 Thin films and Bi prepared by magnetron sputtering 2 O 2 Se film has good matching. And the threshold voltage of the prepared transistor is positive, and the current switching ratio is greater than 10 5 Therefore, if Bi 2 O 2 Se and HfO 2 It can be prepared by magnetron sputtering at the same time, which has a great promoting effect on the development of field effect transistors.

[0021] Embodiment 1:

[0022] In this embodiment, a sapphire substrate with a diameter of 2 inches is used. 2 O 2 The thickness of Se film is 4.5nm, and HfO 2 The film thickness is 15nm. The source, drain and gate electrode material is Ni, and its thickness is 40nm.

[0023] The specific steps are as follows:

[0024] 1. Cleaning the sapphire substrate

[0025] The sapphire substrate was ultrasonically cleaned with acetone for 10 minutes, taken out and placed in anhydrous ethanol for 10 minutes of ultrasonic cleaning, then taken out and placed in deionized water for 10 minutes of ultrasonic cleaning, and then taken out and blown dry with a nitrogen gun for later use.

[0026] 2. Magnetron sputtering Bi 2 O 2 Se thin film

[0027] Fix the dried sapphire substrate prepared in step 1 above on the wafer stage of the magnetron sputtering equipment. 2 O 2 Se target is fixed in the RF sputtering target position, and Bi 2 O 2 The purity of the Se target was 99.9%, the thickness was 3 mm, and the diameter was 50.8 mm. The distance between the target and the substrate was adjusted to 7.2 cm. The pressure in the chamber was pumped to 5 × 10 - 5Pa, the RF sputtering power was adjusted to 20W, the target temperature of the temperature controller was adjusted to 600℃, and when the chamber temperature rose to 600℃, the Ar gas flow rate was adjusted to 40 standard ml / min, where the purity of the Ar gas used was 99.995%. After the pressure in the chamber was adjusted to 2-3Pa, ignition was started, and then the pressure in the chamber was adjusted to 0.45Pa, and sputtering was started. The sputtering time was 68 seconds, and samples were taken after the chamber was cooled to room temperature. The prepared Bi 2 O 2 Raman spectroscopy characterization of Se films Figure 1 shown.

[0028] 3. Preparation of Bi 2 O 2 Se channel

[0029] a. Spin-coat the photoresist on the sample surface in step 2 above and bake at 120°C for 2 minutes for curing.

[0030] b. Place the sample in a above under a custom mask for UV exposure for 7 seconds. After exposure, develop in a developer for 45 seconds. After development, rinse with deionized water and blow dry with a nitrogen gun for later use.

[0031] c. Place the dried sample in b above into a reactive ion etcher, use a mechanical pump to pump the pressure in the chamber to 3.5 Pa, and then use a molecular pump to pump the pressure in the chamber to 8×10 -4 Pa, set the ion source power to 20 W, use 99.995% pure Ar gas as etching gas, the gas flow rate to 10 standard ml / min, and the etching time to 150 seconds.

[0032] d. Soak the sample after etching in c in acetone for 60 minutes, and then continue to soak it in acetone for 5 minutes to remove Bi 2 O 2 The photoresist attached to the Se channel was ultrasonically cleaned with anhydrous ethanol and deionized water for 5 minutes respectively, and then dried with a nitrogen gun for later use.

[0033] 4. Preparation of Source and Drain Electrodes

[0034] a. Spin-coat the surface of the sample prepared in step 3 above with photoresist and bake at 120°C for 2 minutes for curing.

[0035] b. Place the baked sample in a above under a customized mask and use UV lithography to define the Bi 2 O 2 The Se channel forms an ohmic contact source electrode and a drain electrode, wherein the UV exposure time is 7 seconds, and after the exposure, the sample is placed in a developer for 45 seconds.

[0036] c. Fix the sample prepared in b above on the magnetron sputtering stage, and place the Ni target on the DC sputtering target position, where the Ni target has a purity of 99.9%, a thickness of 3 mm, and a diameter of 50.8 mm. Adjust the distance between the target and the substrate to 7.2 cm, and use a mechanical pump and a molecular pump to pump the pressure in the chamber to 5×10 -4 Pa, adjust the DC sputtering power to 80W, adjust the Ar gas flow rate to 40 standard ml / min, wherein the Ar gas purity is 99.995%, at room temperature, adjust the air pressure in the chamber to 2-3Pa, ignite, and then adjust the air pressure in the chamber to 0.65Pa, start sputtering, the sputtering time is 15 minutes, and the thickness of the sputtered Ni electrode is 40nm.

[0037] d. Soak the sample prepared in c above in acetone for 60 minutes, then continue to soak it in acetone for 5 minutes, ultrasonically soak it in anhydrous ethanol and deionized water for 5 minutes, and finally blow dry it with a nitrogen gun for later use.

[0038] 5. Magnetron sputtering HfO 2 Dielectric layer

[0039] The sample prepared in step 4 was fixed on the stage of the magnetron sputtering equipment. 2 The target is fixed in the RF sputtering target position, where HfO 2 The purity of the target material is 99.9%, the thickness is 3 mm, and the diameter is 50.8 mm. The distance between the target material and the substrate is adjusted to 7.2 cm. The pressure in the chamber is pumped to 5×10 -5 Pa, the RF sputtering power was adjusted to 80 W, the Ar gas flow rate was adjusted to 40 standard ml / min at room temperature, and O 2 The gas flow rate was adjusted to 10 standard ml / min, with Ar and O 2 The purity is 99.995%. After the air pressure in the chamber is adjusted to 2-3Pa, the glow is started. After the air pressure in the chamber is adjusted to 0.65Pa, sputtering begins. The sputtering time is 3 hours. Due to the long sputtering time, in order to prevent the target material from overheating and cracking, the glow must be extinguished every 1 hour of sputtering, and the glow must be re-ignited and sputtered after cooling for 10 minutes.

[0040] 6. Preparation of gate electrode

[0041] a. Spin-coat the surface of the sample prepared in step 5 above with photoresist and bake at 120°C for 2 minutes for curing.

[0042] b. Place the sample prepared in step a above under a customized mask and define the gate electrode pattern using UV photolithography technology, wherein the UV exposure time is 7 seconds. After exposure, place the sample in a developer and develop for 45 seconds.

[0043] c. Fix the sample prepared in b above on the magnetron sputtering stage, and place the Ni target on the DC sputtering target position, where the Ni target has a purity of 99.9%, a thickness of 3 mm, and a diameter of 50.8 mm. Adjust the distance between the target and the substrate to 7.2 cm, and use a mechanical pump and a molecular pump to pump the pressure in the chamber to 5×10 -4 Pa, adjust the DC sputtering power to 80W, adjust the Ar gas flow rate to 40 standard ml / min, wherein the Ar gas purity is 99.995%, at room temperature, adjust the air pressure in the chamber to 2-3Pa, ignite, and then adjust the air pressure in the chamber to 0.65Pa, start sputtering, the sputtering time is 15 minutes, and the thickness of the sputtered Ni electrode is 40nm.

[0044] d. Soak the sample prepared in c above in acetone for 60 minutes, then continue to soak it in acetone for 5 minutes, then sonicate it in anhydrous ethanol and deionized water for 5 minutes respectively, and finally blow dry it with a nitrogen gun to complete the preparation of the device.

[0045] 7. Test the device in a semiconductor parameter analyzer.

[0046] The transistor device prepared in this embodiment is shown in FIG. Figure 2 As shown, the performance is Figure 3 As shown in the figure, it can be seen that the transistor exhibits n-type semiconductor characteristics. When a negative voltage is applied to the gate, the drain current is very small and is in the off state. When a positive voltage is applied to the gate, the drain current increases and is in the on state. The switch ratio exceeds 10 5 .

[0047] Embodiment 2:

[0048] The other processes of this embodiment are the same as those of embodiment 1, except that the HfO prepared by magnetron sputtering technology in step 5 is 2 The dielectric layer is prepared by atomic layer deposition. The preparation method is as follows:

[0049] Use 99.9% pure nitrogen as carrier gas, tetra(dimethylamino)hafnium [(CH3)2N]4Hf as hafnium source, and ultrapure water as oxygen source. The background vacuum is higher than 0.01 Torr, the carrier gas flow rate is 8 standard ml / min during deposition, the sample heating temperature is adjusted to 200°C, the hafnium source heating temperature is adjusted to 75°C, and 300 cycles are set. After the deposition is completed, the sample is taken out for use.

[0050] The performance of the transistor prepared in this embodiment is as follows Figure 4As shown in the figure, it can be seen that compared with the preparation of HfO by magnetron sputtering technology 2 Dielectric layer, HfO prepared by atomic layer deposition 2 The threshold voltage of the dielectric layer transistor is negative, and the current switching ratio decreases.

[0051] Embodiment 3:

[0052] The other processes of this embodiment are the same as those of Embodiment 1, except that the materials for preparing the electrodes in Step 4 and Step 6 are adjusted to Ag and Cu.

[0053] The performance of the transistor prepared in this embodiment is as follows Figure 5 As shown in the figure, it can be seen that compared with the preparation of Ni electrode by magnetron sputtering technology, the use of Ag film as electrode ( Figure 5 The transistor current switching ratio in Figure a is slightly reduced to 10 4 , using Cu film as electrode ( Figure 5 The transistor in Figure b) is affected by the heavy doping of Cu, so the off-state current of the transistor is large and the current switch ratio is small, which is 10 3 .

Claims

1. A method for preparing wafer-level Bi2O2Se / HfO2 thin film transistors by full magnetron sputtering, characterized in that: The steps include: Step 1: Using Bi2O2Se target as target, magnetron sputtering is performed on a clean substrate to prepare Bi2O2Se film; Step 2: Using ultraviolet lithography to define the channel pattern on the Bi2O2Se film prepared in step 1, and using Ar ion etching or reactive ion etching to remove the excess film to form a Bi2O2Se channel array; Step 3: Deposit Ni thin film as source and drain electrodes on the Bi2O2Se channel array using magnetron sputtering technology; Step 4: Prepare HfO2 thin film as gate dielectric layer by magnetron sputtering technology; Step 5: Deposit a Ni film on the gate dielectric layer as a gate electrode using magnetron sputtering technology.

2. The method according to claim 1, characterized in that In step 1, the thickness of the Bi2O2Se film is 4~10 nm, and the magnetron sputtering temperature is 400~600 ℃.

3. The method according to claim 1, characterized in that In step 4, the thickness of the HfO2 film is 15-60 nm, the magnetron sputtering temperature is room temperature, and the HfO2 film is prepared by magnetron sputtering technology using HfO2 as a target material.

4. The method according to claim 1, characterized in that In step 3 and step 5, the thickness of the Ni film is 10-100 nm, the magnetron sputtering temperature is room temperature, and the Ni film is deposited by magnetron sputtering technology using Ni as a target.