Two-dimensional contact Bi2O2Se semiconductor thin film transistor and manufacturing method thereof

By using thicker Bi2O2Se as a contact electrode in two-dimensional semiconductor devices to replace traditional metal contact, the Schottky barrier problem is solved, the device performance and manufacturing process matching is improved, and high-performance and low-cost Bi2O2Se-based electronics are achieved. Level integrated circuit manufacturing.

CN119008703APending Publication Date: 2024-11-22NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066365.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Due to the Schottky barrier problem caused by metal contact in traditional two-dimensional semiconductor devices, the electrical performance of the device is reduced, and the manufacturing process matching and cost are high, making it difficult to achieve industrial production.

Method used

Thicker Bi2O2Se is used as the contact electrode to replace traditional metal contacts, and Bi2O2Se thin film transistors are prepared by vacuum magnetron sputtering and atomic layer deposition technology to form a full two-dimensional contact structure to improve the matching of the electrode and channel material.

Benefits of technology

It significantly improves the quality of the contact interface, reduces the Fermi pinning effect, improves transistor performance, reduces manufacturing costs, and achieves electronic-grade integrated circuit manufacturing with scale-cost-performance balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008703A_ABST
    Figure CN119008703A_ABST
Patent Text Reader

Abstract

The invention discloses a two-dimensional contact Bi2O2Se semiconductor thin film transistor and a manufacturing method thereof. The transistor sequentially comprises a substrate, a Bi2O2Se thin film, a source electrode, a drain electrode, a gate dielectric layer and a gate electrode from bottom to top, and the source electrode, the drain electrode and the gate electrode all adopt the Bi2O2Se thin film. The comprehensive two-dimensional contact Bi2O2Se thin film field effect transistor with excellent performance is successfully constructed by utilizing the high Fermi level degeneracy characteristic of the thick Bi2O2Se and the semiconductor characteristic of the thin Bi2O2Se, and compared with a Bi2O2Se field effect transistor using conventional metal as a contact electrode, the comprehensive two-dimensional contact Bi2O2Se thin film field effect transistor has the advantages that the contact resistance can be remarkably reduced, and the performance of the Bi2O2Se thin film field effect transistor is improved. And a smaller off-state current and a higher current switch ratio are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor thin films and devices, and in particular relates to a two-dimensional contact Bi2O2Se semiconductor thin film transistor and a manufacturing method thereof. Background Art

[0002] In recent years, wafer-level synthesis and device processing technology of two-dimensional semiconductors have made great progress and have been applied to advanced electronic and optoelectronic devices. At present, the two-dimensional materials that are widely studied include graphene, black phosphorus and transition metal sulfides. Although these materials show excellent electrical properties and application value, there are also some unavoidable shortcomings that hinder the industrial production of two-dimensional semiconductors, such as the zero band gap of graphene, the environmental instability of black phosphorus and the low mobility of transition metal sulfides. Moreover, the performance of electronic devices based on two-dimensional materials is always subject to low-quality metal semiconductor contacts, so it is still challenging to develop a two-dimensional electronic device with high-quality contacts.

[0003] As a new type of quasi-two-dimensional semiconductor material, Bi2O2Se has extremely outstanding environmental stability, ultra-high electron mobility and excellent optoelectronic properties. It is considered to be a promising alternative to traditional two-dimensional materials and can be used in high-performance logic devices and memory devices. Unlike bulk silicon and other two-dimensional materials, Bi2O2Se has thickness-related electrical property changes. Thinner Bi2O2Se exhibits typical n-type semiconductor behavior, while thicker Bi2O2Se exhibits metal-like conductor behavior. At present, electronic devices based on Bi2O2Se all use traditional metal contacts, which will cause some unavoidable defects, resulting in significant Schottky barriers on the contact interface, reducing the electrical performance of the device. The full two-dimensional contact Bi2O2Se semiconductor thin film transistor provided by the present invention can significantly improve the quality of the contact interface, reduce the Fermi pinning effect, and improve transistor performance compared to traditional devices. Summary of the invention

[0004] The purpose of the present invention is to provide a two-dimensional contact Bi2O2Se semiconductor thin film transistor and a preparation method thereof, using thicker Bi2O2Se to replace traditional metal as a contact electrode, improving the matching between the electrode and the channel material, and significantly improving the device performance.

[0005] In a first aspect, the present invention provides a two-dimensional contact Bi2O2Se semiconductor thin film transistor, which comprises, from bottom to top, a substrate, a Bi2O2Se thin film, a source electrode, a drain electrode, a gate dielectric layer and a gate electrode.

[0006] Preferably, the substrate is a rigid substrate selected from any one of Si, sapphire, mica or quartz glass, and has a size of 1 to 2 inches.

[0007] Preferably, the gate dielectric layer is a ZrO2 film with a thickness of 10 to 60 nm.

[0008] Preferably, the thickness of the Bi2O2Se film is 4 to 10 nm.

[0009] Preferably, the source electrode, the drain electrode and the gate electrode are all made of Bi2O2Se thin film with a thickness of 40 to 60 nm.

[0010] In a first aspect, the present invention further provides a method for mass-producing the transistor according to the first aspect, comprising the following steps:

[0011] Step 1: Using Bi2O2Se target as target, vacuum magnetron sputtering is performed on a clean substrate at a sputtering temperature of 600°C to prepare Bi2O2Se film;

[0012] Step 2: The Bi2O2Se film prepared in step 1 is used to define the channel pattern using ultraviolet lithography technology, and the excess film is removed using Ar ion etching or reactive ion etching to form a Bi2O2Se channel array;

[0013] Step 3: Using vacuum magnetron sputtering to deposit Bi2O2Se thin films as source and drain electrodes on the Bi2O2Se channel array at room temperature;

[0014] Step 4: Atomic layer deposition technology is then used to prepare a ZrO2 film as a gate dielectric layer;

[0015] Step 5: Deposit a Bi2O2Se thin film on the gate dielectric layer as a gate electrode using vacuum magnetron sputtering.

[0016] Compared with the prior art, the present invention has the following advantages and technical effects:

[0017] Compared with the traditional two-dimensional thin film transistor, the full two-dimensional contact Bi2O2Se semiconductor thin film transistor proposed in the present invention can avoid the barrier difference and work function mismatch caused by the traditional metal-two-dimensional material contact, improve the transistor performance, improve the matching of the manufacturing process, and reduce the manufacturing cost. It can realize the manufacture of Bi2O2Se-based electronic-grade integrated circuits with balanced scale, cost and performance, which has important scientific significance and engineering value.

[0018] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0020] Figure 1 This is an optical photograph of a wafer-level Bi2O2Se thin film prepared on a sapphire substrate in Example 1 of the present invention;

[0021] Figure 2 Raman characterization of the wafer-level Bi2O2Se film prepared on a sapphire substrate in Example 1 of the present invention;

[0022] Figure 3 A schematic diagram of the structure of a Bi2O2Se semiconductor thin film transistor prepared in Example 1 of the present invention;

[0023] Figure 4 is an optical microscope image of a transistor prepared in Example 1 of the present invention;

[0024] Figure 5 The transfer characteristic curve of the transistor prepared in Example 1 of the present invention;

[0025] Figure 6 The transfer characteristic curve of the transistor prepared in Example 2 of the present invention;

[0026] Figure 7 This is the transfer characteristic curve of the transistor prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] The present application is further described below in conjunction with specific embodiments.

[0028] It should be noted that the terms such as "upper", "lower", "left", "right", "middle", etc. cited in this specification are only for the convenience of description and are not used to limit the scope of implementation. Changes or adjustments to their relative relationships should be regarded as the scope of implementation of this application without substantially changing the technical content.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.

[0030] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0031] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.

[0032] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.

[0033] Figure 3 The schematic diagram of the structure of the Bi2O2Se semiconductor thin film transistor provided by the present invention includes: an Al2O3 substrate 1, a Bi2O2Se thin film channel 2, a Bi2O2Se contact electrode 3, a ZrO2 dielectric layer 4, and a Bi2O2Se gate electrode 5.

[0034] Embodiment 1:

[0035] In this embodiment, the thickness of the Bi2O2Se thin film channel is 5.5 nm, and the dielectric layer is made of ZrO2 with a thickness of 30 nm.

[0036] In the transistor prepared in this example, the substrate is 2-inch sapphire, and the source, drain and gate electrodes are all Bi2O2Se with a thickness of 40nm.

[0037] The specific steps are as follows:

[0038] 1. Magnetron sputtering method for growing wafer-level Bi2O2Se thin films

[0039] Using Bi2O2Se target as target material and cleaned sapphire substrate as substrate, vacuum magnetron sputtering was performed. The vacuum degree during sputtering was higher than 5×10 -5 Pa, and the substrate was heated to 600°C using a resistance wire heating device. High-purity Ar gas (99.995%) was used as the sputtering gas, the sputtering pressure was adjusted to 0.4 Pa, the RF power was adjusted to 20 W, and the sputtering time was 68 seconds. After the sputtering was completed, the chamber was cooled to room temperature, and the sample was taken out for use. The optical photograph of the obtained Bi2O2Se film is shown in Figure 1. Figure 1 As shown, Raman characterization is as follows Figure 2 shown.

[0040] 2. Thin film etching

[0041] a) Spin-coating the sample with photoresist, and then placing the sample on a heating table at 120° C. for 2 minutes to cure the photoresist;

[0042] b) Using UV lithography, the custom mask was used to expose the area outside the channel, and then the sample was soaked in a developer for 35 seconds, then rinsed with deionized water, and then dried with a nitrogen gun;

[0043] c) Place the dried sample into the etcher and turn on the mechanical pump and molecular pump to draw the vacuum to 8×10 -4 Pa, the ion source power was adjusted to 20 watts, Ar gas with a purity of 99.995% was used as the etching gas, the gas flow rate was adjusted to 10 standard ml / min, and the etching time was 2 minutes;

[0044] d) Soak the etched sample in acetone for 40 minutes to remove residual photoresist, then clean the sample with anhydrous ethanol, take it out and blow dry it with nitrogen for later use.

[0045] 3. Preparation of Source and Drain Electrodes

[0046] a) spin coating the etched sample with photoresist, and heating and curing the photoresist;

[0047] b) Use a customized mask to perform a second photolithography, align the layer mark, expose the source electrode and drain electrode areas, then soak the sample in the developer for 35 seconds, then rinse the sample with deionized water and blow dry with a nitrogen gun;

[0048] c) Depositing Bi2O2Se using the same method as step 1, except that the substrate temperature is room temperature and the deposition time is 495 seconds;

[0049] d) Soak the sample in acetone for 40 minutes to remove residual glue, and then clean the sample with anhydrous ethanol to obtain source and drain electrodes.

[0050] 4. Atomic layer deposition of ZrO2 dielectric layer

[0051] Use 99.9% pure nitrogen as carrier gas, tetra(dimethylamino)hafnium [(CH3)2N]4Hf as hafnium source, and ultrapure water as oxygen source. The background vacuum is higher than 0.01 Torr, the carrier gas flow rate is 8 standard ml / min during deposition, the sample heating temperature is adjusted to 200°C, the hafnium source heating temperature is adjusted to 75°C, and 300 cycles are set. After the deposition is completed, the sample is taken out for use.

[0052] 5. Gate Electrode Preparation

[0053] a) spin coating the sample with photoresist, and heating and curing the photoresist;

[0054] b) Perform the third photolithography using a customized mask. After aligning the layer mark, expose the gate electrode area, then soak the sample in the developer for 35 seconds, then rinse the sample with deionized water and blow dry with a nitrogen gun;

[0055] c) Depositing Bi2O2Se using the same method as step 1, except that the substrate temperature is room temperature and the deposition time is 495 seconds;

[0056] d) Soak the sample in acetone for 40 minutes to remove residual glue, and then clean the sample with anhydrous ethanol to complete the device preparation.

[0057] 6. Test the device in a semiconductor parameter analyzer.

[0058] The optical microscope image of the transistor prepared in this embodiment is as follows Figure 4 As shown, the transistor performance is Figure 5 As shown in the figure, when a negative voltage is applied to the gate, the drain current is very small, about 140pA, and is in the off state. When a positive voltage is applied to the gate, the drain current increases and is in the on state, showing obvious n-type semiconductor behavior, and the switching ratio is about 7.1×10 3 .

[0059] Embodiment 2:

[0060] The other processes of this embodiment are the same as those of Embodiment 1, except that the source electrode, the drain electrode and the gate electrode are all made of metal Ag with a thickness of 60 nm.

[0061] The specific steps are as follows:

[0062] a) Using high-purity Ag target (99.99%) as the target material, the photolithography-finished sample is placed in a magnetron sputtering coating apparatus for vacuum sputtering. The vacuum degree during the sputtering process is higher than 1×10 -4 High-purity Ar gas (99.995%) was used as the sputtering gas, the sputtering gas pressure was adjusted to 0.5 Pa, the DC power was adjusted to 20 W, and the sputtering time was 300 seconds.

[0063] b) Soak the sample in acetone for 40 minutes to remove residual glue, and then clean the sample with anhydrous ethanol to complete the device preparation.

[0064] The performance of the transistor prepared in this embodiment is as follows Figure 6 As shown, Figure 6 It can be seen that the off-state current of the device is about 7.4nA and the on-off ratio is about 2×10 2 .

[0065] Embodiment 3:

[0066] The other processes of this embodiment are the same as those of Embodiment 1, except that the source electrode, the drain electrode and the gate electrode are all made of metal Al with a thickness of 60 nm.

[0067] The specific steps are as follows:

[0068] a) Using high-purity Al target (99.99%) as the target material, the photolithography-finished sample was placed in a magnetron sputtering coater for vacuum sputtering. The vacuum degree during the sputtering process was higher than 1×10 -4 High-purity Ar gas (99.995%) was used as the sputtering gas, the sputtering gas pressure was adjusted to 0.4 Pa, the DC power was adjusted to 20 W, and the sputtering time was 300 seconds.

[0069] b) Soak the sample in acetone for 40 minutes to remove residual glue, and then clean the sample with anhydrous ethanol to complete the device preparation.

[0070] The performance of the transistor prepared in this embodiment is as follows Figure 7 As shown, Figure 7 It can be seen that the off-state current of the device is about 0.6nA and the on-off ratio is about 3×10 3 .

[0071] The performance of the transistors obtained in Examples 1-3 is summarized in Table 1.

[0072] Table 1

[0073]

[0074] From Table 1, it can be found that the device using thicker Bi2O2Se as the contact electrode has the best performance. Compared with the device composed of traditional metal contact electrodes, the two-dimensional contact Bi2O2Se semiconductor thin film transistor has lower off-state current, higher switching ratio, and smaller positive threshold voltage. When the device is used in logic devices, it can significantly reduce device power consumption and achieve more stable circuit operation.

[0075] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.

Claims

1. A two-dimensional contact Bi2O2Se semiconductor thin film transistor, characterized in that: From bottom to top, it includes: substrate, Bi2O2Se film, source electrode, drain electrode, gate dielectric layer and gate electrode.

2. The transistor according to claim 1, wherein: The substrate is a rigid substrate selected from any one of Si, sapphire, mica or quartz glass, and has a size of 1 to 2 inches.

3. The transistor according to claim 1, wherein: The gate dielectric layer is a ZrO2 film with a thickness of 10~60 nm.

4. The transistor according to claim 1, wherein: The thickness of Bi2O2Se film is 4~10 nm.

5. The transistor according to claim 1, wherein: The source electrode, drain electrode and gate electrode are all made of Bi2O2Se thin film with a thickness of 40~60nm.

6. A method for mass-producing the transistor according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: Using Bi2O2Se target as target, vacuum magnetron sputtering is performed on a clean substrate at a sputtering temperature of 600°C to prepare Bi2O2Se film; Step 2: The Bi2O2Se film prepared in step 1 is used to define the channel pattern using ultraviolet lithography technology, and the excess film is removed using Ar ion etching or reactive ion etching to form a Bi2O2Se channel array; Step 3: Using vacuum magnetron sputtering to deposit Bi2O2Se thin films as source and drain electrodes on the Bi2O2Se channel array at room temperature; Step 4: Atomic layer deposition technology is then used to prepare a ZrO2 film as a gate dielectric layer; Step 5: Deposit a Bi2O2Se thin film on the gate dielectric layer as a gate electrode using vacuum magnetron sputtering.