Method for synthesizing 2H / 1T 'TMD heterogeneous phase junction and device based on method

The 2H and 1T′MoS2 layers were grown on the substrate by CVD method, forming a 2H/1T′MoS2 heterogeneous phase junction, which solved the problem of difficult to achieve high purity and interface clarity in the prior art, and achieved high-performance MoS2 heterogeneous phase Junction devices, suitable for optoelectronic applications.

CN119008727APending Publication Date: 2024-11-22CITY UNIV OF HONG KONG SHENZHEN RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311351252.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-21
Filing Date
2023-10-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing methods are difficult to achieve high purity and clear van der Waals interfaces when preparing 2H/1T′MoS2 heterogeneous junctions, and large-scale preparation depends on harsh post-processing processes, affecting device performance.

Method used

By using chemical vapor deposition (CVD) method, a transition metal compound is mixed with a chalcogen element powder, multi-stage heating and gas flow treatment are carried out, and 2H and 1T′MoS2 layers are grown on the substrate to form a 2H/1T′MoS2 heterogeneous phase junction. , avoid post-processing steps.

Benefits of technology

The growth of high-purity 2H/1T′MoS2 heterogeneous junctions is achieved, demonstrating excellent rectification capabilities and fast response times, suitable for optoelectronic applications without additional post-processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008727A_ABST
    Figure CN119008727A_ABST
Patent Text Reader

Abstract

A method of synthesizing a 2H / 1T'transition metal dichalcogenide (TMD) heterogeneous phase junction is provided. The synthesis of the vertical 2H / 1T 'MoS2 heterogeneous phase junction is realized, a 2H MoS2 single layer grows on a mica substrate by using pure Ar carrier gas, and then the 1T' MoS2 nanobelt grows on the 2H MoS2 single layer by changing the carrier gas from pure Ar to mixed gas of Ar and H2. The integrated device based on the 2H / 1T 'MoS2 heterogeneous phase structure shows typical rectification characteristics, has a current rectification ratio of more than 102, and realizes the responsivity of 1.07 A / W at 532 nm under the ultralow dark current of less than 10 <-11 > A. Due to the excellent characteristics, the 2H / 1T 'MoS2 heterogeneous phase structure becomes an unprecedented candidate material of a rectifier and a photoelectric detector in the future. More importantly, the provided synthesis method can selectively grow two phases of MoS2, and further paves a way for improving the performance of an electronic device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to transition metal dichalcogenide (TMD) heterojunctions. More specifically, the present invention relates to a chemical vapor deposition (CVD) method for growing a 2H / 1T' molybdenum disulfide (MoS2) heterojunction. Background Art

[0002] Two-dimensional (2D) TMDs have attracted extensive attention due to their diverse properties, ranging from insulators, semiconductors, semimetals to metals. When different 2D materials are stacked vertically, the advantages of multiple materials can be combined. With the development of phase engineering of nanomaterials (PEN), the crystalline phase of TMDs has become one of the most important structural features besides size, morphology and symmetry, determining the intrinsic properties of TMDs. Different from thermodynamically stable phases, many non-conventional phases have distinct properties.

[0003] For example, 2H MoS2 usually shows semiconducting properties, while 1T and 1T′ MoS2 usually show metallic properties. Heterojunctions, especially heterophase junctions, have attracted increasing attention due to their potential to act as high-performance devices such as rectifiers, detectors, and transistors for energy storage, electrocatalysis, and optoelectronics applications. Many studies have shown that the coexistence of semiconductor and metallic polycrystalline phases in 2D heterophase junctions is very important for improving carrier mobility, thereby enhancing the overall performance of the device.

[0004] 1T′MoS2 has a semi-metallic phase with high electrical conductivity, and 1T′MoS2 in contact with metal shows a lower contact barrier compared to 2H MoS2. The 2H / 1T′MoS2 heterojunction structure shows a clear van der Waals interface, which is conducive to fast photoresponse time and high photoelectric responsivity.

[0005] Existing methods for obtaining MoS2 heterojunctions are usually based on manual stacking and local phase transitions, which inevitably introduce contaminants and interface defects. In addition, existing methods for large-scale preparation of MoS2 heterojunctions strongly rely on post-processing processes such as laser irradiation, lithium intercalation, and chemical doping, which have complex and harsh reaction conditions and poor controllability. However, it is still challenging to directly epitaxially (or in situ) grow high-purity metastable 1T′MoS2 with clear van der Waals interfaces on 2H MoS2 heterojunctions because the energy required for the formation of the 1T′ phase is much higher than that of the 2H phase. Summary of the invention

[0006] According to an embodiment of the first aspect of the present invention, a method for synthesizing a 2H / 1T′TMD heterojunction is provided. The method comprises: mixing a transition metal compound powder with a first chalcogen element powder to form a first mixture; placing the first mixture in a CVD furnace, filling the CVD furnace with argon gas, and then heating the first mixture to a first temperature; injecting a first hydrogen-argon mixed gas flow into the CVD furnace, maintaining the first mixture at the first temperature for a first period of time to form a first precursor; mixing the first precursor with a second chalcogen element powder to form a second mixture; placing the second mixture in a CVD furnace, filling the CVD furnace with argon gas, and then heating the second mixture to a second temperature, injecting a second hydrogen-argon mixed gas flow into the CVD furnace, and maintaining the second mixture at the second temperature for a second period of time to form a second precursor; placing a substrate on top of the second precursor; placing the second precursor and the substrate in a CVD furnace, filling the CVD furnace with argon gas, and then heating the second precursor and the substrate to a growth temperature; injecting an argon gas flow into the CVD furnace, maintaining the second precursor and the substrate at the growth temperature for a first growth period to grow 2H on the substrate. TMD layer; injecting a third hydrogen-argon mixed gas flow into the CVD furnace, maintaining the second precursor and the substrate at the growth temperature for a second growth period to grow a 1T′TMD layer on the grown 2H TMD layer; and rapidly cooling the substrate on which the 2H / 1T′TMD heterojunction is grown.

[0007] According to another embodiment of the first aspect of the present invention, the method further includes, before heating the first mixture, grinding the first mixture in an agate mortar, transferring the ground first mixture into a first alumina crucible, and placing the first alumina crucible at a center position of the CVD furnace.

[0008] According to another embodiment of the first aspect of the present invention, the method further includes, before heating the second mixture, grinding the second mixture in an agate mortar, transferring the second mixture into a second alumina crucible, and placing the second alumina crucible at a center position of the CVD furnace.

[0009] According to another embodiment of the first aspect of the present invention, the method also includes transferring the second precursor into a quartz crucible before placing the substrate on the second precursor, and placing the quartz crucible at a center position of the CVD furnace before heating the substrate and the second precursor.

[0010] According to another embodiment of the first aspect of the present invention, the substrate is a fluorophlogopite substrate or a sapphire substrate.

[0011] According to another embodiment of the first aspect of the present invention, the hydrogen-argon flow ratio in the first hydrogen-argon mixed gas flow is 1:9; the first temperature range is 400 to 500 degrees Celsius, and the first time period ranges from 1 to 2 hours.

[0012] According to another embodiment of the first aspect of the present invention, the hydrogen-argon flow ratio in the second hydrogen-argon mixed gas flow is 1:9; the second temperature range is 400 to 500 degrees Celsius, and the second time period ranges from 1 to 2 hours.

[0013] According to another embodiment of the first aspect of the present invention, the hydrogen-argon flow ratio in the third hydrogen-argon mixed gas flow is 2:8; the growth temperature ranges from 750 to 800 degrees Celsius, and the first growth period range and the second growth period range are both 4 to 6 minutes.

[0014] According to another embodiment of the first aspect of the present invention, the transition metal compound powder is a molybdenum compound powder, and the first and second chalcogenide powders are both sulfur powders, so that the 2H / 1T′TMD heterojunction grown on the substrate is a 2H / 1T′ molybdenum sulfide heterojunction.

[0015] According to another embodiment of the first aspect of the present invention, the molybdenum compound powder is potassium molybdate (K2MoO4) powder.

[0016] According to an embodiment of the second aspect of the present invention, a device based on a 2H / 1T′TMD heterojunction is provided. The device comprises: a substrate; a 2H / 1T′TMD heterojunction deposited on the substrate, comprising a 1T′-TMD region and a 2H-TMD region; and a pair of electrodes respectively connected to the 1T′-TMD region and the 2H-TMD region.

[0017] According to another embodiment of the second aspect of the present invention, the 1T′-TMD region is formed of 1T′-MoS 2 crystals, and the 2H-TMD region is formed of 2H-MoS 2 crystals.

[0018] According to another embodiment of the second aspect of the present invention, the substrate is a SiO2 / Si substrate.

[0019] According to another embodiment of the second aspect of the present invention, the electrode is made of Cr / Au layer.

[0020] It is gratifying that in the synthesized 2H / 1T′MoS2 heterojunction, the grown 1T′MoS2 nanoribbons can extend over the area of ​​the 2HMoS2 monolayer, which makes it possible to directly fabricate devices using the prepared heterojunction without any additional post-processing. Therefore, the present invention provides a new strategy for the field of phase engineering, which can also be used to prepare other heterojunctions.

[0021] Devices based on 2H / 1T′TMD heterojunctions (e.g., devices based on 2H / 1T′MoS2 heterojunctions) prepared using the CVD method provided by the present invention exhibit excellent rectification capabilities, high responsiveness, and fast response time, indicating that 2H / 1T′MoS2 heterojunctions have great potential in future optoelectronic applications. In addition, 2H / 1T′MoS2 heterojunctions can be used as anisotropic conductors and microscopic battery catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The embodiments of the present invention will be described in more detail below with reference to the accompanying drawings, in which:

[0023] Figures 1A to 1C The three main stages of a general method for growing a 2H / 1T′TMD heterojunction according to some embodiments of the present invention are shown;

[0024] Figure 2A Schematic diagram and typical optical images of the prepared 2H / 1T′MoS2 heterojunction are shown ( Figure 2A illustrations); Figure 2B and Figure 2C Optical images of the synthesized 2H / 1T′MoS2 heterojunction at other different scales are shown;

[0025] Figure 3A and Figure 3B Transmission electron microscopy (TEM) images of the prepared 2H / 1T′MoS2 heterojunction are shown;

[0026] Figure 4 Schematic diagram showing the prepared 2H / 1T′MoS2 heterojunction;

[0027] Figure 5 shows the aberration-corrected high-angle dark field (HAADF) scanning transmission electron microscopy (STEM) cross-sectional image of the prepared 2H / 1T′MoS2 heterojunction;

[0028] Fig. 6A and Figure 6B High-resolution (HR) TEM images of 2H MoS2 and 1T′MoS2 regions are shown, respectively;

[0029] Fig. 7A and Figure 7B Atomic-resolution HAADF-STEM images of 2H MoS2 and 1T′MoS2 are shown, respectively; Fig. 7A and Figure 7B The insets show the selected area electron diffraction (SAED) patterns of 2H MoS2 and 1T′MoS2 regions, respectively;

[0030] Figure 8 Dark-field HRTEM image of 2H / 1T′MoS2 heterojunction is shown;

[0031] 9A to 9C The element distribution images of Mo L signal and SK signal of 2H / 1T′MoS2 heterojunction and the overlapped image of Mo L and SK signals are shown respectively;

[0032] Fig.10 The Raman spectra of 2H MoS2 layer, 1T′MoS2 layer and mica substrate are shown;

[0033] Fig.11A and Fig. 11B The angle-dependent Raman intensities of the 2H MoS2 and 1T′MoS2 regions are shown, respectively;

[0034] Fig.12 The photoluminescence (PL) spectra of the 2H MoS2 and 1T′MoS2 regions are shown;

[0035] Fig.13A and Fig. 13B Thickness measurements of the 2H MoS2 and 1T′MoS2 regions are shown, respectively;

[0036] Fig.14 An atomic force microscopy (AFM) image of the 2H / 1T′MoS2 heterojunction is shown;

[0037] Fig.15A and Fig. 15B The spectra of Mo3d and S2p orbitals of micro-area X-ray photoelectron spectroscopy (XPS) of 2H MoS2 and 1T′MoS2 regions are shown, respectively;

[0038] Fig.16A and Fig. 16B The XPS K 2p orbital spectra of the 2H MoS2 and 1T′MoS2 regions are shown, respectively;

[0039] Fig.17A and Fig. 17B Raman scanning images of 2H MoS2 and 1T′MoS2 regions are shown respectively;

[0040] Fig.18 shows a schematic diagram of a device based on a 2H / 1T′TMD heterojunction, according to some embodiments of the present invention;

[0041] Fig.19 The typical optical images of 2H / 1T′MoS2 heterojunction devices are shown respectively;

[0042] Fig. 20The corresponding AFM images of 2H / 1T′MoS2 heterojunction devices are shown;

[0043] Fig.21A The transfer characteristic curve of the 2H / 1T′MoS2 heterojunction device is shown. Fig. 21B shows the I at different gate voltages ds -V ds Characteristic curve;

[0044] Fig.22A The transfer characteristic curves of the comparative 2H MoS2 device are shown. Fig. 22B shows the I at different gate voltages ds -V ds Characteristic curve;

[0045] Fig.23A The 2H / 1T′MoS2 heterojunction device has a power of 3.52 mW / cm 2 Input power of 532nm laser for different V ds Time-resolved photocurrent curves of bias voltage; Fig. 23B Shows Fig.23A A magnified view of the curve of ;

[0046] Fig.24 The optical switching characteristics of the 2H / 1T′MoS2 heterojunction device for different wavelengths are shown. DETAILED DESCRIPTION

[0047] In the following description, embodiments of the present invention are described as preferred examples. It is apparent to those skilled in the art that modifications, including additions and / or substitutions, may be made without departing from the scope and spirit of the present invention. In order not to confuse the present invention, certain specific details may be omitted. However, the writing of this disclosure enables those skilled in the art to practice the teachings herein without excessive experimentation.

[0048] According to one aspect of the present invention, a general method for growing 2H / 1T′TMD heterojunctions is provided. The method adopts a one-pot synthesis strategy, including Figures 1A to 1C The three main stages are shown.

[0049] refer to Figure 1AIn the first stage, a transition metal compound powder and a first chalcogen element powder are mixed to form a first mixture. The first mixture is ground in an agate mortar and then transferred to a first alumina crucible. The first alumina crucible containing the first mixture is then placed in the center of a CVD furnace. Argon gas is filled into the CVD furnace, and then the first mixture is heated to a first temperature; a first hydrogen-argon mixed gas flow is injected into the CVD furnace, and the first mixture is maintained at the first temperature for a first period of time to form a first precursor. The first precursor is then naturally cooled to room temperature.

[0050] refer to Figure 1B In the second stage, the first precursor is mixed with the second chalcogenide powder to form a second mixture. The second mixture is transferred to a second alumina crucible. The second alumina crucible containing the second mixture is then placed in the center of the CVD furnace. Argon is filled into the CVD furnace, and then the second mixture is heated to a second temperature. A second hydrogen-argon mixed gas flow is injected into the CVD furnace, and the second mixture is maintained at a second temperature for a second period of time to form a second precursor. The second precursor is then naturally cooled to room temperature. refer to Figure 1C , in the third stage, the second precursor is loaded into a quartz crucible, and then a substrate is placed on top of the second precursor. The quartz crucible and the substrate are then placed in the center of the CVD furnace. The CVD furnace is filled with argon gas, and then the second precursor and the substrate are heated to the growth temperature. An argon flow is injected into the CVD furnace, and the second precursor and the substrate are maintained at the growth temperature for a first growth period to grow a 2H TMD layer on the substrate. A third hydrogen-argon mixed flow is injected into the CVD furnace, and the second precursor and the substrate are maintained at the growth temperature for a second growth period to grow a 1T′TMD layer on the grown 2H TMD layer. The substrate on which the 2H / 1T′TMD heterojunction is grown is then taken out of the CVD furnace and rapidly cooled.

[0051] Synthesis of 2H / 1T′MoS2 Heterojunction

[0052] The synthesis method of the vertical 2H / 1T′MoS2 heterojunction is achieved by simply changing the carrier gas. Briefly, a monolayer of 2H MoS2 is first grown on a mica substrate under a pure argon atmosphere. Then, by changing the carrier gas from pure argon to an argon-hydrogen mixed gas, 1T′MoS2 nanoribbons are continuously grown on top of the monolayer of 2H MoS2, thereby forming a 2H / 1T′ heterojunction.

[0053] In a typical 2H / 1T′MoS2 heterogeneous phase synthesis process, 600 milligrams (mg) of potassium molybdate (K2MoO4) and 600 milligrams (mg) of sulfur (S) powder were mixed and ground in a mortar for 10 minutes. The resulting homogeneous mixture was then transferred to an alumina crucible, which was placed in the center of a quartz furnace tube. Subsequently, the quartz furnace tube was evacuated and filled with argon three times to remove the air inside the tube. After flushing the pipeline with a pure argon flow (flow rate of 500 standard cubic centimeters per minute (sccm)) for 10 minutes, the furnace was heated to 450°C and injected with a hydrogen-argon mixed flow (hydrogen flow rate of 10 s.ccm and argon flow rate of 90 s.ccm) for 1.5 hours. After cooling to room temperature, the product was taken out and mixed with 600 mg of sulfur powder, and then the resulting uniform mixture was loaded into an alumina crucible, and the alumina crucible was placed in the center of the furnace. Next, the quartz furnace tube was evacuated and filled with argon three times to remove the air in the tube. After flushing the pipeline with a pure argon flow (flow rate of 500 s.ccm) for 10 minutes, the furnace was heated to 450°C and injected with a hydrogen-argon mixed flow (hydrogen flow rate of 10 s.ccm and argon flow rate of 90 s.ccm). Gas flow rate is 90s.ccm) and maintained for 1.5 hours. After the reaction is completed, the obtained precursor is taken out when the furnace is naturally cooled to room temperature. Subsequently, 10 mg of the precursor is loaded in a quartz crucible, and a newly peeled fluorphlogopite substrate is covered on the top of the precursor. The quartz crucible is then placed in the center of the furnace. After the quartz furnace tube is evacuated and filled with argon three times, the furnace is heated to 780°C under a pure argon flow (flow rate of 10s.ccm). Afterwards, a hydrogen-argon mixed flow (hydrogen flow rate of 20s.ccm and argon flow rate of 80s.ccm) is injected and maintained for 5 minutes. After the reaction is completed, the power of the furnace is turned off, and the mica substrate on which the 2H / 1T′MoS2 heterojunction is synthesized is quickly removed from the heating zone.

[0054] Characterization of 2H / 1T′MoS2 Heterojunction

[0055] Figure 2A Schematic diagram and typical optical images of the prepared 2H / 1T′MoS2 heterojunction are shown ( Figure 2A Figure 3 (inset), where 1T′MoS2 on the top and 2H MoS2 on the bottom can be clearly distinguished by their optical contrast. Figure 2B and 2C Other optical images of the synthesized 2H / 1T′MoS2 heterojunction at different scales are shown. The heterojunction consists of triangular 2H MoS2 monolayers and 1T′MoS2 nanoribbons.

[0056] The size of 1T′MoS2 nanoribbons can exceed that of 2H MoS2, which allows us to directly fabricate devices based on the grown heterojunctions, thus avoiding redundant processing steps with the opportunity to lose material. In addition, compared with the traditional two-step method, this one-pot synthesis strategy uses only a single solid source, which can avoid interface contamination.

[0057] Figure 3A and 3B The TEM image of the prepared 2H / 1T′MoS2 heterojunction is shown. The morphology of the 2H / 1T′MoS2 heterojunction is similar to Figure 4 The same schematic diagram is shown.

[0058] like Figure 5 As shown, the HAADF-STEM cross-sectional image of the prepared 2H / 1T′MoS2 heterojunction shows the clear boundaries of the heterojunction along the atomic boundaries without obvious atomic mixing or defects.

[0059] refer to Fig. 6A and 6B , 2H MoS2( Fig. 6A ) and 1T′MoS2( Figure 6B ) clearly shows the distinct atomic structures between the distorted octahedral 1T′ phase and the triangular prism-shaped 2H phase. This feature is also evident in the atomically resolved HAADF-STEM image of 2H MoS2 ( Fig. 7A Atomic-resolution HAADF-STEM image of neutralized 1T′MoS2 ( Figure 7B As previously reported, 1T′MoS2 clearly shows a zigzag chain structure. In addition, the SAED pattern of 2HMoS2 ( Fig. 7A Compared with the hexagonally symmetrical spots shown in the inset of Figure 2, the SAED pattern of 1T′MoS2 ( Figure 7B The inset of Figure 3 shows periodic spots with rectangular symmetry.

[0060] Figure 8 Dark-field HRTEM image of the 2H / 1T′MoS2 heterojunction is shown. Figures 9A to 9C The elemental scanning images of the Mo L signal, SK signal and the overlapped Mo L and SK signals in the 2H / 1T′MoS2 heterojunction are shown respectively. As shown in the figure, the signals of Mo and S are evenly distributed in the 2H / 1T′MoS2 heterojunction. These results confirm that the 2H / 1T′MoS2 heterojunction has high purity, good crystallinity and clear heterojunction lines.

[0061] Fig.10 Raman spectra of 2H MoS2, 1T′MoS2 and mica substrates are shown. Fig.10The inset shows a typical optical image of the 2H / 1T′MoS2 heterojunction. As shown in the figure, the two typical Raman peaks (385 and 404 cm -1 ) are different, five different Raman peaks (148 cm -1 、206cm -1 、277cm -1 、323cm -1 and 403cm -1 ). 2H MoS2( Fig.11A ) and 1T′MoS2( Fig. 11B ) also shows obvious differences in the angle-dependent Raman intensity. The 2H MoS2 monolayer shows no angle dependence.

[0062] Fig.12 The PL spectra of 1T′MoS2 and 2H MoS2 are shown. 1T′MoS2 shows metallic properties without absorption peaks, while 2H MoS2 exhibits semiconductor properties with a strong and sharp exciton peak at 677nm, which is a typical PL characteristic spectrum of monolayer MoS2.

[0063] Fig.13A and 13B The thickness measurements of 1T′MoS2 and 2H MoS2 regions are shown separately. Combined with AFM images ( Fig.14 ) and the distance between the two typical Raman peaks of 2H MoS2, which can further prove that the CVD-grown 2H MoS2 is a single layer.

[0064] Fig.15A and 15B Micro-area XPS spectra of Mo 3d and S2p orbitals in 2H MoS2 and 1T′ MoS2 regions are shown, respectively. Fig.16A and 16B The XPS spectra of K 2p orbitals in the 2H MoS2 and 1T′MoS2 regions are shown, respectively. The Mo 3d peaks of 1T′-MoS2 are located at 227.9 and 231 eV, corresponding to the 3d 5 / 2 and 3D 3 / 2 orbital, while the Mo 3d peak of 2H MoS2 shifted to higher binding energies (229.2 and 232.4 eV). A similar shift was observed for the binding energy of the S2p orbital. In addition, no K 2p signal was detected, indicating that K has been completely removed from the synthesized heterojunction. 2H MoS2 ( Fig.17A ) and 1T′MoS2( Fig. 17B ) demonstrates the high crystal quality and phase purity of the prepared heterojunction.

[0065] Fabrication of 2H / 1T′MoS2 Heterojunction Devices

[0066] Since large-scale 1T′MoS2 nanoribbons can be grown outside the 2H MoS2 region, the heterojunction prepared by this synthetic method can be directly used without additional post-processing steps to fabricate devices based on 2H / 1T′MoS2 heterojunctions.

[0067] In one embodiment, in order to manufacture a device based on a 2H / 1T′MoS2 heterojunction, the 2H / 1T′MoS2 heterojunction synthesized by the synthesis method provided by the present invention is first transferred to a silicon dioxide / silicon (SiO2 / Si) substrate. First, a thin film of polymethyl methacrylate (PMMA495, A8, Microchem) is coated on a fluorophlogopite substrate on which a 2H / 1T′MoS2 heterojunction is grown at a rotation speed of 4000 rpm, and then baked on an 80°C hot plate for 30 minutes. The mica substrate is then immersed in deionized water. After the film falls off the mica substrate, the film is transferred to a freshly cleaned 300 nanometer (nm) thick SiO2 / Si substrate and baked on an 80°C hot plate for 10 minutes to promote the adhesion of the 2H / 1T′MoS2 heterojunction on the SiO2 / Si substrate. The SiO2 / Si substrate with the 2H / 1T'MoS2 heterojunction attached was immersed in acetone for 20 minutes to remove PMMA, leaving the 2H / 1T'MoS2 heterojunction on the SiO2 / Si substrate. Finally, a chromium / gold (Cr / Au) (e.g., Cr(8nm) / Au(32nm)) electrode was fabricated on the synthesized monolayer crystal using a typical photolithography process.

[0068] Characterization of 2H / 1T′MoS2 Heterojunction Devices

[0069] Fig.19 A typical optical image of a device based on a 2H / 1T′MoS2 heterojunction is shown. Fig. 20 The corresponding AFM images in show that the device has a clean surface. Fig.21A The transfer characteristic curve in the circuit shows typical n-type semiconductor characteristics, and its on-off ratio is about 10 5 .exist Fig. 21B The output characteristics (Ids-Vds) at different gate voltages (ranging from 0V to 40V) show that I ds With V g Increase gradually.

[0070] It is worth noting that compared with pure 2H MoS2 ( Fig.22A and Fig. 22B), the transfer characteristic curve and gate-controlled output curve of the device based on 2H / 1T′MoS2 heterojunction also show obvious current rectification characteristics, further confirming that a Schottky junction is formed at the interface of 1T′ and 2HMoS2.

[0071] In addition, due to the presence of the Schottky junction, the device shows good optoelectronic performance. Under negative drain-source bias and gate voltage, a 10 -11 Ultra-low dark current of Class A. Fig.23A The device showed a 3.52 mW / cm 2 Input power of 532nm laser for different V ds Time-resolved photocurrent curve of bias voltage. As the drain-source voltage increases, the photocurrent gradually increases, and a high responsivity of up to 1.07A / W is achieved at a drain-source bias voltage of -0.5V. Fig.23A It can also be seen from all the curves that the photocurrent rises rapidly under laser irradiation and then drops sharply when the laser is turned off. Due to the limited resolution of our measurement equipment, the measured drop time is less than 24 milliseconds (see Fig. 23B ). In addition, Fig.24 The photo-switching properties shown for different wavelengths also show high responsivity and fast response time. These encouraging results highlight the potential of 2H / 1T′MoS2 heterojunction phototransistors for practical applications.

[0072] Embodiments may be selected and described to best explain the principles of the present invention and its practical application, so that other technical personnel in the art can understand the various embodiments of the present invention and various modifications suitable for specific purposes. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it should be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless otherwise specifically noted herein, the order and grouping of operations are not restrictive. Although the devices disclosed herein have been described with reference to specific structures, shapes, materials, material compositions and relationships, etc., these descriptions and illustrations are not restrictive. Modifications may be made to adapt specific situations to the purpose, spirit and scope of the present disclosure. All of these modifications are intended to fall within the scope of the appended claims.

Claims

1. A method for synthesizing a 2H / 1T′TMD heterojunction, comprising: mixing a transition metal compound powder with a first chalcogen element powder to form a first mixture; Putting the first mixture into a CVD furnace, filling the CVD furnace with argon gas, and then heating the first mixture to a first temperature; injecting a first hydrogen-argon mixed gas flow into the CVD furnace, and maintaining the first mixture at the first temperature for a first period of time to form a first precursor; Mixing the first precursor with a second chalcogen element powder to form a second mixture; placing the second mixture into a CVD furnace, filling the CVD furnace with argon gas, then heating the second mixture to a second temperature, injecting a second hydrogen-argon mixed gas flow into the CVD furnace, and maintaining the second mixture at the second temperature for a second period of time to form a second precursor; placing a substrate on top of the second precursor; placing the second precursor and the substrate into a CVD furnace, filling the CVD furnace with argon gas, and then heating the second precursor and the substrate to a growth temperature; Injecting an argon gas flow into the CVD furnace, maintaining the second precursor and the substrate at the growth temperature for a first growth period to grow a 2H TMD layer on the substrate; Injecting a third hydrogen-argon mixed gas flow into the CVD furnace, maintaining the second precursor and the substrate at the growth temperature for a second growth period to grow a 1T′TMD layer on the grown 2H TMD layer; and The substrate on which the 2H / 1T′TMD heterojunction is grown is rapidly cooled.

2. The method of claim 1 further includes, before heating the first mixture, grinding the first mixture in an agate mortar, transferring the ground first mixture into a first alumina crucible, and placing the first alumina crucible at a center position of the CVD furnace.

3. The method according to claim 1 further includes, before heating the second mixture, grinding the second mixture in an agate mortar, transferring the second mixture to a second alumina crucible, and placing the second alumina crucible at a center position of the CVD furnace.

4. The method of claim 1 further comprising transferring the second precursor into a quartz crucible before placing the substrate on top of the second precursor, and placing the quartz crucible at a central position of the CVD furnace before heating the substrate and the second precursor.

5. The method according to claim 1, wherein the substrate is a fluorophlogopite substrate or a sapphire substrate.

6. The method of claim 1, wherein the hydrogen-argon flow ratio in the first hydrogen-argon mixed gas flow is 1:9; the first temperature range is 400 to 500 degrees Celsius, and the first time period ranges from 1 to 2 hours.

7. The method of claim 1, wherein the hydrogen-argon flow ratio in the second hydrogen-argon mixed gas flow is 1:9; the second temperature range is 400 to 500 degrees Celsius, and the second time period ranges from 1 to 2 hours.

8. The method of claim 1, wherein the hydrogen-argon flow ratio in the third hydrogen-argon mixed gas flow is 2:8; the growth temperature ranges from 750 to 800 degrees Celsius, and the first growth period ranges from 4 to 6 minutes and the second growth period ranges from 4 to 6 minutes.

9. The method of claim 1, wherein the transition metal compound powder is a molybdenum compound powder, and the first and second chalcogenide powders are both sulfur powders, so that the 2H / 1T′TMD heterojunction grown on the substrate is a 2H / 1T′ molybdenum sulfide heterojunction.

10. The method of claim 9, wherein the molybdenum compound powder is potassium molybdate (K2MoO4) powder.

11. A 2H / 1T′TMD heterojunction device manufactured by the method of claim 1, comprising: substrate; A 2H / 1T′TMD heterojunction deposited on the substrate, comprising a 1T′-TMD region and a 2H-TMD region; as well as A pair of electrodes are respectively connected to the 1T′-TMD region and the 2H-TMD region.

12. The 2H / 1T′TMD heterojunction device of claim 11, wherein the 1T′-TMD region is formed of 1T′-MoS2 crystals, and the 2H-TMD region is formed of 2H-MoS2 crystals.

13. The 2H / 1T′TMD heterojunction device of claim 11, wherein the substrate is a SiO2 / Si substrate.

14. The 2H / 1T'TMD heterojunction device of claim 11, wherein the electrode is made of a Cr / Au layer.